Large-size zinc oxide nanoflower as well as preparation method and application thereof
Through the hydrothermal reaction and calcination method of zinc oxide nanoparticles with alkaline aqueous solution, the problem of purity and morphology control of zinc oxide nanoflowers is solved, and the efficient preparation of large-size nanoflowers is achieved, suitable for high-performance materials and Gas separation technology.
Patent Information
- Application Number
- CN202411097298.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-11-12
Smart Images

Figure CN118929733A_ABST
Abstract
Description
Technical Field
[0001] The present invention specifically relates to a large-size zinc oxide nanoflower and a preparation method and application thereof. Background Art
[0002] Zinc oxide is a multifunctional material with broad application prospects. It has attracted attention in many fields due to its unique physical and chemical properties. Zinc oxide has a wide band gap, high electron mobility and excellent chemical stability, which makes it important for applications in optoelectronic devices, gas sensors and catalysts. However, traditional zinc oxide materials have limitations in some applications, especially in areas with special requirements for material thickness and surface area, such as separation materials. In order to meet the special needs of these fields, zinc oxide nanoflowers with ultra-thin lamellar structures have emerged.
[0003] The preparation methods of zinc oxide nanoflowers are mainly concentrated in two categories: gas phase method and solution method. Gas phase methods such as chemical vapor deposition and molecular beam epitaxy can prepare high-purity and high-crystalline quality zinc oxide films. However, the process has high energy consumption, complex and expensive equipment, and harsh process conditions. The solution method includes hydrothermal method, sol-gel method and chemical bath deposition, which has the advantages of simple equipment, mild process and easy control and has attracted mainstream attention.
[0004] However, the existing solution method preparation route still has some shortcomings. For example, the preparation process is cumbersome and requires the addition of some polymers and chelating agents to assist in the formation of nanosheet structures. Any slight deviation may lead to the formation of irregular morphology or impurities, and precise control of the nanoflower structure is difficult to achieve. Furthermore, the reaction takes a long time, and the resulting zinc oxide nanoflowers have low purity and low crystallinity, and their size and morphology are difficult to achieve precise control, affecting the overall performance and repeatability of the material.
[0005] In the prior art, there is also a process for preparing zinc oxide nanosheet clusters by using a zinc salt solution and an alkali for precipitation reaction. However, the size of the zinc oxide nanosheet clusters prepared by this process is not large enough, and its application scenarios are still limited. For example, it cannot be used in the field of gas molecule separation technology with high requirements. Summary of the invention
[0006] In view of the shortcomings and deficiencies of the prior art, the purpose of the present invention is to provide a method for preparing large-sized zinc oxide nanoflowers, which can prepare large-sized zinc oxide nanoflowers and is easy to control the structure of the zinc oxide nanoflowers. The zinc oxide nanoflowers can be used for the preparation of MOF membranes, and the membranes can be used for the separation of gas molecules.
[0007] In order to achieve the above object, the technical solution adopted by the present invention is:
[0008] A method for preparing zinc oxide nanoflowers, the preparation method comprising the following steps: 1) dispersing zinc oxide nanoparticles in an alkaline aqueous solution to obtain a mixed solution; 2) subjecting the mixed solution to a hydrothermal reaction, and obtaining sodium metazincate nanoflowers after solid-liquid separation, wherein the sodium metazincate nanoflowers include a plurality of sodium metazincate nanosheets, and the particle size of the sodium metazincate nanoflowers is 2 to 20 μm; 3) calcining the sodium metazincate nanoflowers to obtain the zinc oxide nanoflowers, wherein the zinc oxide nanoflowers include a plurality of zinc oxide nanosheets, and the particle size of the zinc oxide nanoflowers is 2 to 20 μm.
[0009] In the present invention, the particle size of the nanoflower refers to the size in the SEM image. Since the sizes of different nanoflowers may vary slightly, the particle size of the nanoflower obtained by a specific solution may be a small range value.
[0010] In the prior art, zinc oxide nanosheets or nanoflowers are usually synthesized by precipitation or hydrothermal reaction of a zinc salt solution and an alkali, but the size of the obtained zinc oxide nanosheets or nanoflowers is not large enough, and the structure of the nanoflowers or nanosheets is difficult to accurately control, which easily leads to irregular morphology, and is also difficult to be used in the preparation of MOF membranes, and thus difficult to be used in high-requirement technical fields such as gas molecule separation. The inventors of the present application have found through research that zinc oxide nanoparticles are used as raw materials, and are subjected to hydrothermal reaction with alkaline aqueous solution. The zinc oxide nanoparticles are first subjected to morphological transformation while reacting to generate a large-sized nanoflower precursor containing multiple nanosheets, that is, a nanoflower with a chemical composition of sodium metazincate, and then the precursor is calcined. During the calcination process, the morphology of the nanoflower remains unchanged, and the chemical composition changes to generate a stable zinc oxide nanoflower, which also has a large size and its morphology is easy to accurately control.
[0011] In some embodiments, the average particle size of the zinc oxide nanoparticles is 50 to 300 nm. Preferably, the average particle size of the zinc oxide nanoparticles is 100 to 200 nm. Using this preferred range, zinc oxide nanoflowers with larger particle sizes can be obtained.
[0012] In some embodiments, the alkaline aqueous solution is a sodium bicarbonate aqueous solution. Compared with traditional alkaline substances such as sodium hydroxide or potassium hydroxide, the use of sodium bicarbonate is more conducive to the precise control of the zinc oxide nanoflower structure.
[0013] In some embodiments, the molar concentration of the alkaline aqueous solution is 0.2-0.5 mol / L.
[0014] In some embodiments, in step 1), the dispersion is achieved by stirring at room temperature.
[0015] In some embodiments, the stirring time is 10-60 min.
[0016] In some embodiments, the zinc oxide nanoparticles are transferred into an alkaline aqueous solution under stirring conditions of 50 to 150 r / min, and stirring is continued for 15 to 30 min to obtain the mixed solution.
[0017] In some embodiments, the molar ratio of the zinc oxide nanoparticles to sodium bicarbonate is 1:1 to 4. The molar ratio of the zinc oxide nanoparticles to sodium bicarbonate will affect the size of the zinc oxide nanoflowers, and large-sized zinc oxide nanoflowers can be obtained within the aforementioned range.
[0018] In some embodiments, the temperature of the hydrothermal reaction is 60-150° C., preferably 60-80° C. In the aforementioned temperature range, especially in the preferred temperature range, zinc oxide nanoflowers with better morphology can be obtained.
[0019] In some embodiments, the hydrothermal reaction time is 2 to 6 hours. Using the above reaction time range, zinc oxide nanoflowers with more controllable sheet thickness and better morphology can be obtained.
[0020] In some embodiments, the hydrothermal reaction is carried out under stirring, preferably, the stirring speed is 5 to 15 r / min. Stirring can make the reaction more uniform and controllable, and the structural transformation of zinc oxide nanoparticles to precursor nanoflowers is more thorough.
[0021] In some embodiments, in step 2), the solid-liquid separation is achieved by centrifugation.
[0022] In some embodiments, the preparation method further comprises washing and drying after the solid-liquid separation.
[0023] In some embodiments, washing is performed by centrifugation with deionized water for 3 to 5 times.
[0024] In some embodiments, the drying temperature is 60-80°C.
[0025] In some embodiments, the drying time is 2 to 5 hours.
[0026] In some embodiments, the plurality of sodium metazincate nanosheets have a length of 0.5 to 2 μm and a thickness of 10 to 100 nm.
[0027] In some embodiments, the length of the plurality of zinc oxide nanosheets is 0.5 to 2 μm, and the thickness is 10 to 100 nm. During the calcination process, the physical structure of the nanoflowers is not changed, and only the chemical composition is changed.
[0028] In some embodiments, the calcination temperature is 300-500°C.
[0029] In some embodiments, the calcination time is 1 to 3 hours.
[0030] The present invention also provides zinc oxide nanoflowers prepared by the above preparation method.
[0031] The present invention also provides a method for preparing zinc oxide nanosheets, comprising the step of ultrasonically treating zinc oxide nanoflowers, and the preparation method further comprises the step of preparing zinc oxide nanoflowers by adopting the above-mentioned method for preparing zinc oxide nanoflowers.
[0032] The present invention also provides a zinc oxide nanosheet prepared by the above-mentioned method for preparing the zinc oxide nanosheet.
[0033] Furthermore, the zinc oxide nanosheet has a length of 0.5 to 2 μm and a thickness of 10 to 100 nm.
[0034] The present invention also provides the use of the zinc oxide nanosheets for preparing MOF membranes. The zinc oxide nanosheets of the present invention have multifunctional application prospects, and their high specific surface area, flatness, reaction activity and excellent photocatalytic performance make them show significant advantages in the fields of high-performance separation materials, catalytic materials and environmentally friendly materials.
[0035] Due to the application of the above technical solution, the present invention has the following advantages compared with the prior art:
[0036] (1) The present invention uses zinc oxide nanoparticles as raw materials and conducts a hydrothermal reaction with an alkaline aqueous solution. The zinc oxide nanoparticles are first subjected to a morphological transformation during the reaction to generate a large-sized nanoflower precursor containing multiple nanosheets, i.e., a nanoflower whose chemical composition is sodium metazincate. The precursor is then calcined. During the calcination process, the morphology of the nanoflower remains unchanged, while the chemical composition is transformed to generate a stable zinc oxide nanoflower. The zinc oxide nanoflower also has a large size and its morphology is easy to accurately control.
[0037] (2) The preparation method of the zinc oxide nanoflower of the present invention is simple to operate, has simple process steps, has low requirements on equipment, and has cheap and readily available raw materials, which can significantly reduce the cost and energy consumption of preparation and is easy to produce in large quantities. By adjusting the molar ratio of zinc element to bicarbonate and the temperature and time of the hydrothermal reaction, the sheet thickness and morphology of the zinc oxide nanoflower can be simply and accurately controlled.
[0038] (3) The preparation method of the present invention can obtain zinc oxide nanoflowers with high yield and high purity. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 This is the SEM image of the sodium metazincate nanoflowers prepared in Example 1;
[0040] Figure 2This is the SEM image of the zinc oxide nanoflower prepared in Example 1;
[0041] Figure 3 The XRD patterns of sodium metazincate nanoflowers and zinc oxide nanoflowers prepared in Example 1 are compared;
[0042] Figure 4 This is a SEM image of the monolayer zinc oxide nanosheet prepared in Example 1;
[0043] Figure 5 The TGA graphs of the sodium metazincate nanoflowers and zinc oxide nanoflowers prepared in Example 1 are compared;
[0044] Figure 6-8 They are SEM images of zinc oxide nanoflowers prepared in Examples 2-4 respectively;
[0045] Figure 9-11 They are respectively the SEM image, XRD pattern and nitrogen adsorption isotherm of the MOF crystal prepared in Example 12;
[0046] Figure 12-14 The SEM image, XRD image and gas separation performance test of the MOF membrane material prepared in Example 13 are respectively;
[0047] Fig.15 This is the SEM image of the zinc oxide nanoflowers prepared in Comparative Example 1. DETAILED DESCRIPTION
[0048] The technical solution of the present invention is described in detail below in conjunction with specific embodiments so that those skilled in the art can better understand and implement the technical solution of the present invention, but the present invention is not limited to the scope of the examples.
[0049] Example 1
[0050] This embodiment provides a zinc oxide nanoflower and a zinc oxide nanosheet, and the preparation steps thereof are as follows:
[0051] (1) Weigh 0.005 mol of commercially available zinc oxide nanoparticles (particle size 100 nm) and disperse them in 50 mL of a pre-prepared sodium bicarbonate aqueous solution with a concentration of 0.2 mol / L (the molar ratio of zinc oxide nanoparticles to sodium bicarbonate is 1:2). Then, turn on a mechanical stirrer and stir at a set speed of 50 r / min for 15 min to obtain a milky white colloid.
[0052] (2) The milky white colloid prepared in step (1) was transferred into a polytetrafluoroethylene liner, which was then sealed and placed in a homogeneous reactor equipped with stirring. The hydrothermal reaction was continued for 2 hours at a reaction temperature of 80° C. and a rotation speed of 5 r / min.
[0053] (3) After the reaction was completed, the reactor was cooled to room temperature naturally, and the product was collected by high-speed centrifugation (8000 r / min, 10 min), and washed with deionized water three times. The product was then placed in a 60°C forced air drying oven and dried for 3 h to obtain white sodium metazincate nanoflowers, as shown in the SEM image. Figure 1 As shown in Figure 1, its particle size is 3 microns, and it is composed of a flake structure with a length of 1 micron and a thickness of 10 to 10 nanometers. Its XRD pattern is shown in Figure 1. Figure 3 As shown in the figure, the ZnO precursor is
[0054] (4) The sodium metazincate nanoflowers obtained in step (3) were placed in a muffle furnace, heated to 400° C. at a heating rate of 5° C. / min and calcined for 2 h to obtain zinc oxide nanoflowers, the SEM image of which is shown in FIG. Figure 2 As shown, its size is 4-5 μm, the nanoflower includes a plurality of zinc oxide nanosheets, and the thickness of the zinc oxide nanosheets is 20 nm. The yield of zinc oxide nanoflowers is 98%. Powder X-ray diffraction (XRD) pattern ( Figure 3 ) also confirmed that the obtained zinc oxide nanoflowers were highly crystalline zinc oxide. Figure 3 From the comparison of XRD of zinc oxide nanoflowers and sodium metazincate nanoflowers, it can be seen that high-purity zinc oxide nanoflower structure was successfully obtained after calcination treatment.
[0055] (5) The zinc oxide nanoflowers obtained in step (4) were dispersed in 10 mL of deionized water, and after ultrasonic treatment in an ultrasonic cell crusher for 1 h, the product was collected by differential centrifugation and dried at high temperature (60° C.) to obtain a monolayer zinc oxide nanosheet with uniform size. Figure 4 ) shows that the size of the ZnO nanosheets is 1 μm.
[0056] TGA comparison of sodium metazincate nanoflowers and zinc oxide nanoflowers Figure 5 As shown, it can be seen that after calcination, the thermal stability of nanoflowers is significantly improved.
[0057] Embodiment 2-4
[0058] The method is basically the same as Example 1, except that the molar ratio of zinc oxide nanoparticles to sodium bicarbonate in step (1) is adjusted from 1:2 to 1:1, 1:3 and 1:3.5 respectively. The SEM images of the obtained zinc oxide nanoflowers are shown in FIG. Figure 6-8 The sizes of the nanoflowers are shown in Table 1.
[0059] Table 1
[0060]
[0061] Example 5-11
[0062] The method is basically the same as Example 1, except that the temperature and time of the hydrothermal reaction in step (2) are adjusted as shown in Table 2 below. The size of the obtained zinc oxide nanoflowers is also shown in Table 2.
[0063] Table 2
[0064]
[0065] Example 12
[0066] In this example, the zinc oxide nanosheets prepared in Example 1 are converted into MOF crystalline materials, as follows.
[0067] (1) Weigh 0.5 mol of 2-methylimidazole organic ligand and dissolve it in 20 mL of deionized water. Stir the mixture with ultrasonic waves for 5 min to obtain a light yellow clear and transparent aqueous solution.
[0068] (2) The monolithic zinc oxide nanosheets prepared in step 5 of Example 1 are stirred and dispersed in the 2-methylimidazole aqueous solution prepared in step 1.
[0069] (3) After the 2-methylimidazole aqueous solution containing zinc oxide nanosheets obtained in step 2 is transferred to a reactor, the reaction is carried out in a constant temperature oven at 40° C. for 3 h, thereby converting the zinc oxide nanosheets into MOF crystals.
[0070] From the scanning electron microscopy images ( Fig. 9 ) shows that the ZnO nanosheets are successfully transformed into crystals with obvious rhombic dodecahedral morphology, and the powder X-ray diffraction pattern ( Fig.10 , also including the results of reaction time 0.5h, 1h, 2h, and XRD was used to monitor the reaction process) to confirm that the generated crystal is ZIF-8, 77K nitrogen adsorption isotherm ( Fig.11 ) The BET specific surface area of the obtained ZIF-8 crystal was 1503.1 m 2 / g, which is close to the theoretical value of the material.
[0071] Embodiment 13
[0072] In this example, the zinc oxide nanosheets prepared in Example 1 are converted into MOF membrane materials, as follows.
[0073] (1) The monolithic zinc oxide nanosheets prepared in step 5 of Example 1 were dispersed in 50 mL of ethylene glycol to prepare a dispersion with a concentration of 20 mg / L.
[0074] (2) The zinc oxide nanosheets were deposited on the surface of the porous alumina support by vacuum filtration. When 50 mL of ethylene glycol dispersion completely permeated from the upstream to the downstream of the porous alumina, a zinc oxide nanosheet layer with a thickness of 1 μm was obtained on the surface of the support.
[0075] (3) Weigh 1 mol of 2-methylimidazole organic ligand and dissolve it in 25 mL of deionized water. Stir it with ultrasonic for 5 min to obtain a light yellow clear transparent aqueous solution. The solution is then transferred into a 50 mL polytetrafluoroethylene liner.
[0076] (4) After the alumina support with the zinc oxide nanosheet layer deposited thereon obtained in step 2 is vertically placed in the polytetrafluoroethylene liner of step 3, it is placed in a constant temperature oven at 40° C. for reaction for 6 hours, so that the zinc oxide nanosheet layer can be converted into a continuous and dense MOF membrane.
[0077] From the scanning electron microscopy images ( Fig.12 ) shows that the zinc oxide nanosheet layer on the surface of the support is successfully transformed into a continuous crystal film layer, and the powder X-ray diffraction pattern ( Fig.13 ) confirmed that the generated crystal was ZIF-8, and the gas separation performance test ( Fig.14 ) confirmed that the prepared membrane has excellent propylene / propane high-pressure separation performance.
[0078] Comparative Example 1
[0079] The process is basically the same as Example 1, except that the zinc oxide nanoparticles in step (1) are replaced with zinc acetate, which is dissolved in the same sodium bicarbonate aqueous solution, and the subsequent steps of reaction are also carried out in the same manner. The SEM image of the zinc oxide nanoflowers finally obtained is as follows: Fig.15 As shown, it can be seen that its size is 800nm and the sheet thickness is 5nm, that is, its size is smaller than that of Example 1, and there is obvious agglomeration.
[0080] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing zinc oxide nanoflowers, characterized in that: The preparation method comprises the following steps: 1) dispersing zinc oxide nanoparticles in an alkaline aqueous solution to obtain a mixed solution; 2) subjecting the mixed solution to a hydrothermal reaction, and obtaining sodium metazincate nanoflowers after solid-liquid separation, wherein the sodium metazincate nanoflowers include a plurality of sodium metazincate nanosheets, and the particle size of the sodium metazincate nanoflowers is 2 to 20 μm; 3) calcining the sodium metazincate nanoflowers to obtain the zinc oxide nanoflowers, wherein the zinc oxide nanoflowers include a plurality of zinc oxide nanosheets, and the particle size of the zinc oxide nanoflowers is 2 to 20 μm.
2. The method for preparing zinc oxide nanoflowers according to claim 1, characterized in that: The average particle size of the zinc oxide nanoparticles is 50 to 300 nm; and / or, the alkaline aqueous solution is a sodium bicarbonate aqueous solution; and / or, the molar concentration of the alkaline aqueous solution is 0.2 to 0.5 mol / L; and / or, in step 1), the dispersion is achieved by stirring at room temperature.
3. The method for preparing zinc oxide nanoflowers according to claim 2, characterized in that: The molar ratio of the zinc oxide nanoparticles to sodium bicarbonate is 1:1-4.
4. The method for preparing zinc oxide nanoflowers according to claim 1, characterized in that: The temperature of the hydrothermal reaction is 60-150° C.; and / or, the time of the hydrothermal reaction is 2-6 hours; and / or, the hydrothermal reaction is carried out under stirring, preferably, the stirring speed is 5-15 r / min.
5. The method for preparing zinc oxide nanoflowers according to claim 1, characterized in that: In step 2), the solid-liquid separation is achieved by centrifugation; and / or the preparation method further comprises the steps of washing and drying after the solid-liquid separation.
6. The method for preparing zinc oxide nanoflowers according to claim 1, characterized in that: The length of the plurality of sodium metazincate nanosheets is 0.5 to 2 μm, and the thickness is 10 to 100 nm; and / or the length of the plurality of zinc oxide nanosheets is 0.5 to 2 μm, and the thickness is 10 to 100 nm.
7. The method for preparing zinc oxide nanoflowers according to claim 1, characterized in that: The calcination temperature is 300-500° C.; and / or the calcination time is 1-3 hours.
8. Zinc oxide nanoflowers prepared by the method for preparing zinc oxide nanoflowers according to any one of claims 1 to 7.
9. A method for preparing zinc oxide nanosheets, comprising the step of subjecting zinc oxide nanosheets to ultrasonic treatment; characterized in that: The preparation method also includes the step of preparing zinc oxide nanoflowers using the preparation method of zinc oxide nanoflowers according to any one of claims 1 to 7.
10. A zinc oxide nanosheet prepared by the method for preparing zinc oxide nanosheets according to claim 9.
11. Use of the zinc oxide nanosheets according to claim 10 for preparing MOF membranes.