Preparation method and application of zinc germanate material

The preparation of zinc germanate nanowires by thermal method of zinc acetate and germanium oxide in a mixed solvent solved the problems of large energy consumption and complex preparation, and achieved low-cost, high-purity and good electrochemical performance zinc germanate nanowire materials , suitable for large-scale commercial manufacturing.

CN118929735APending Publication Date: 2024-11-12UESTC (SHENZHEN) ADVANCED RES INST +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410904401.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-05
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The preparation of existing zinc germanate materials requires high temperature, large energy consumption, complex preparation procedures, and high cost, which is not conducive to large-scale commercial manufacturing.

Method used

The zinc germanate nanowire was prepared by mixing solvent-heating method of zinc acetate and germanium oxide in deionized water and ethylenediamine.

Benefits of technology

It reduces the cost of raw materials and simplifies operation. The product has high purity and good crystallinity, good electrochemical performance, stable charge and discharge specific capacity, large lithium ion diffusion coefficient, and ideal rate performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118929735A_ABST
    Figure CN118929735A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and application of a zinc germanate material, and relates to the technical field of lithium ion battery materials. The preparation method of the zinc germanate material comprises the following operation steps: dissolving zinc acetate and germanium oxide into deionized water and ethidene diamine, mixing and stirring the two solutions for 15 minutes, transferring the obtained milk white solution into a stainless steel reaction kettle, putting the stainless steel reaction kettle into a drying oven, heating for a period of time, then cooling to room temperature, and filtering to obtain the zinc germanate material. And washing the obtained product with distilled water and absolute ethyl alcohol respectively, carrying out centrifugal filtration, carrying out vacuum drying after filtration, and carrying out high-temperature calcination in an argon atmosphere for a period of time to obtain the product zinc germanate nanowire. According to the invention, the zinc germanate nanowire is synthesized by adopting a method of combining mixed solvent heat with high-temperature calcination; the cost of the raw materials used in the method is low; the method is simple to operate; the reaction conditions are relatively mild, and the product is high in purity, good in crystallinity and uniform in morphology.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of lithium ion battery materials, and in particular to a preparation method and application of a zinc germanate material. Background Art

[0002] With the development of science and technology and changes in the environment, people's demands for energy and environmental protection in their daily lives are getting higher and higher. Traditional fossil energy will produce a lot of carbon emissions during use, which is very unfriendly to the environment, while energy technologies such as solar energy, wind energy, and tidal energy are restricted by time, geography and other factors. Therefore, lithium-ion battery technology, as a secondary battery (rechargeable) with light weight, no memory effect, high energy density and environmental friendliness, has attracted the attention of a large number of researchers. Since its successful commercialization in the 1990s, it has been widely used, such as smart phones, laptops, electric vehicles, etc. The traditional commercial lithium-ion battery negative electrode material is graphite, and its theoretical specific capacity is only 372mAh g-1, which greatly limits the development and application of this technology. Therefore, the development of a new type of high energy density lithium-ion battery negative electrode material is the key to the development and application of lithium-ion battery technology.

[0003] At present, more and more researchers are focusing on the application of germanate and its oxide in the negative electrode of lithium-ion batteries. Song (Adv.Funct.Mater.2015,25,6858–6866) research group of North China Electric Power University studied a material with a layered C3N4 nano Zn2GeO4 particle structure, which has a synergistic effect and its reversible specific capacity can still reach 1370mAh g-1 after 140 cycles. Cao (ACS Appl.Mater.Interfaces 2016,8,1388-1397) research group developed a zinc germanate nanofiber network, which has a continuous, interpenetrating porous structure through electrospinning. The material has high specific capacity, stable cycle performance and excellent rate performance. This is because the porosity promotes the diffusion of electrolytes and shortens the transmission path of lithium ions. Yan (Acs Appl Mater Interfaces, 2016: 31722-31728.)'s research team synthesized zinc germanate nanowires by recrystallization. After 130 cycles at a current density of 0.2A g-1, the reversible specific capacity remained stable at 1075.6mAh g-1, and had good amplification performance.

[0004] Patent application number CN2012105532960A discloses a method for preparing zinc germanate nanowires, but the material preparation requires a relatively high temperature, high energy consumption, a relatively complex preparation procedure, and high costs, which is not conducive to large-scale commercial manufacturing. Summary of the invention

[0005] Technical issues solved

[0006] In view of the shortcomings of the prior art, the present invention provides a preparation method and application of zinc germanate material, which solves the problems that the preparation of the existing material requires high temperature, high energy consumption, complex preparation procedure, high cost, and is not conducive to large-scale commercial manufacturing.

[0007] Technical Solution

[0008] To achieve the above objectives, the present invention is implemented by the following technical scheme: a preparation method and application of zinc germanate material, comprising the following steps:

[0009] S1: Dissolve zinc acetate and germanium oxide in deionized water and ethylenediamine, stir the two solutions separately for 30 minutes until they are completely dissolved, and then mix and stir the two solutions for 15 minutes;

[0010] S2: transferring the milky white solution obtained in S1) into a stainless steel reactor, placing the stainless steel reactor in an oven and heating it for a period of time, and then cooling it to room temperature;

[0011] S3: washing the product obtained in S2) with distilled water and anhydrous ethanol respectively, centrifugally filtering, and vacuum drying after filtering;

[0012] S4: The product obtained after vacuum drying in S3) is placed in an argon atmosphere and calcined at high temperature for a period of time to obtain the product zinc germanate nanowires.

[0013] Preferably, the zinc acetate in S1) has a molecular formula of Zn(Ac)2·2H2O, and its molar ratio to deionized water is 1.5:1-2.5:1.

[0014] Preferably, the germanium oxide in S1) has a molecular formula of GeO2, and its molar ratio to ethylenediamine is 1.5:1-3:1.

[0015] Preferably, the stainless steel reactor in S2) is placed in an oven and heated to 120-180° C., and the constant temperature reaction time is 3-36 hours.

[0016] Preferably, in said S4), the vacuum dried product is placed in an argon atmosphere and calcined at a high temperature of 500-800° C. for 3-9 hours.

[0017] Preferably, when the calcination temperature is 650°C, the nanowire morphology is the most complete. When the temperature is too low, the reaction is incomplete. When the temperature is higher than 650°C, the nanowires agglomerate.

[0018] The invention provides a zinc germanate nanowire material.

[0019] Preferably, the charging platform of the material is around 1.0-1.2 V, and when the current density is 100 mA g -1 After 150 cycles of charge and discharge, the reversible specific capacity is stable at 1190 mAh g -1 , its impedance is small and the lithium ion diffusion coefficient is large; when the current density is 2000mA g -1 When the charge and discharge capacity is stable at 600mAh g -1 When the current density returns to 100mAg -1 When the charge-discharge capacity is reduced to 1000 mAh g -1 The rate performance is ideal.

[0020] The invention provides an application of a zinc germanate nanowire material in a negative electrode of a lithium electronic battery.

[0021] Beneficial Effects

[0022] The present invention has the following beneficial effects:

[0023] (1) The preparation method and application of the zinc germanate material are as follows: the zinc germanate nanowires are synthesized by a mixed solvent thermal method combined with a high temperature calcination method. The raw materials used in the method are low in cost, the method is simple to operate, the reaction conditions are relatively mild, the product has high purity, good crystallinity, and uniform morphology, and its unit cell parameters are consistent with the standard atlas PDF#11-0687.

[0024] (2) The preparation method and application of the zinc germanate material. The ethylenediamine in the present invention plays the dual role of solvent and template agent, which is beneficial to the self-assembly of ions in the reaction system to generate zinc germanate nanowire structure.

[0025] (3) Preparation method and application of the zinc germanate material. The zinc germanate nanowires synthesized by the present invention have good electrochemical properties. The charging platform of the material is around 1.0-1.2V. When the current density is 100mA g -1 After 150 cycles of charge and discharge, the reversible specific capacity is stable at 1190 mAh g -1 , its impedance is small and the lithium ion diffusion coefficient is large. When the current density is 2000mA g -1 When the charge and discharge capacity is stable at 600mAh g -1 When the current density returns to 100 mA g -1 When the charge-discharge capacity is 1000 mAh g -1 Around, the rate performance is ideal.

[0026] Of course, any product implementing the present invention does not necessarily need to achieve all of the advantages described above at the same time. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is a SEM test image of the zinc germanate nanowire material prepared in an embodiment of the present invention;

[0028] Figure 2 This is an XRD test diagram of the zinc germanate nanowire material prepared in an embodiment of the present invention;

[0029] Figure 3 This is a test diagram of the electrochemical performance of the zinc germanate nanowire sample prepared in an embodiment of the present invention;

[0030] Figure 4 The impedance test and Warburg linear fitting diagram of the zinc germanate nanowire sample prepared in the embodiment of the present invention;

[0031] Figure 1 In which, Figure a and Figure b are SEM images of the precursor; Figure c and Figure d are SEM images of the sample synthesized at a calcination temperature of 550°C; Figure e and Figure f are SEM images of the sample synthesized at a calcination temperature of 550°C; Figure g and Figure h are SEM images of the sample synthesized at a calcination temperature of 550°C;

[0032] Figure 2 In the figure, a, b, and c are the charge and discharge curves of ZGO-650, ZGO-550, and ZGO-750, respectively; d is the charge and discharge curves of the three groups of samples at 100 mA g -1 e is the cycle comparison diagram under the current density of ZGO-650 and ; f is the cyclic voltammetry test diagram of ZGO-650, with a scan rate of 0.1mV / S and a voltage range of 0.01-3.0V. DETAILED DESCRIPTION

[0033] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0034] In the description of the present invention, it should be understood that the terms "opening", "upper", "lower", "thickness", "top", "middle", "length", "inside", "all around" and the like indicating orientation or positional relationship are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the components or elements referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as limiting the present invention.

[0035] See also Figure 1-Figure 4 , the present invention provides the following technical solutions:

[0036] Embodiment 1: The present invention provides a technical solution: a preparation method and application of a zinc germanate material, comprising the following steps:

[0037] S1: Stir and mix zinc acetate and deionized water at a molar ratio of 1.5:1-2.5:1, stir and mix germanium oxide and ethylenediamine at a molar ratio of 1.5:1-3:1, stir the two solutions for 30 minutes respectively until they are completely dissolved, and then stir the two solutions for 15 minutes;

[0038] S2: The milky white solution obtained in S1) is transferred to a stainless steel reactor, and the stainless steel reactor is placed in an oven and heated to 120-180° C. for constant temperature reaction for 3-36 hours, and then cooled to room temperature;

[0039] S3: washing the product obtained in S2) with distilled water and anhydrous ethanol respectively, centrifugally filtering, and vacuum drying after filtering;

[0040] S4: the product obtained after vacuum drying in S3) is placed in an argon atmosphere and calcined at 550° C. for 3-9 hours to obtain zinc germanate nanowires.

[0041] Embodiment 2: The present invention provides a technical solution: a preparation method and application of a zinc germanate material, comprising the following steps:

[0042] S1: Stir and mix zinc acetate and deionized water at a molar ratio of 1.5:1-2.5:1, stir and mix germanium oxide and ethylenediamine at a molar ratio of 1.5:1-3:1, stir the two solutions for 30 minutes respectively until they are completely dissolved, and then stir the two solutions for 15 minutes;

[0043] S2: The milky white solution obtained in S1) is transferred to a stainless steel reactor, and the stainless steel reactor is placed in an oven and heated to 120-180° C. for constant temperature reaction for 3-36 hours, and then cooled to room temperature;

[0044] S3: washing the product obtained in S2) with distilled water and anhydrous ethanol respectively, centrifugally filtering, and vacuum drying after filtering;

[0045] S4: the product obtained after vacuum drying in S3) is placed in an argon atmosphere and calcined at 650° C. for 3-9 hours to obtain zinc germanate nanowires.

[0046] Example 3: Please refer to Figure 1-Figure 4 The present invention provides a technical solution: a preparation method and application of zinc germanate material, comprising the following steps:

[0047] S1: Stir and mix zinc acetate and deionized water at a molar ratio of 1.5:1-2.5:1, stir and mix germanium oxide and ethylenediamine at a molar ratio of 1.5:1-3:1, stir the two solutions for 30 minutes respectively until they are completely dissolved, and then stir the two solutions for 15 minutes;

[0048] S2: The milky white solution obtained in S1) is transferred to a stainless steel reactor, and the stainless steel reactor is placed in an oven and heated to 120-180° C. for constant temperature reaction for 3-36 hours, and then cooled to room temperature;

[0049] S3: washing the product obtained in S2) with distilled water and anhydrous ethanol respectively, centrifugally filtering, and vacuum drying after filtering;

[0050] S4: the product obtained after vacuum drying in S3) is placed in an argon atmosphere and calcined at 750° C. for 3-9 hours to obtain zinc germanate nanowires.

[0051] Table 1 shows the kinetic parameters of the zinc germanate nanowires prepared in the examples of the present invention.

[0052] Electrodes <![CDATA[R u (Oh)]]> <![CDATA[R ct (Oh)]]> <![CDATA[C dl (mF / cm 2 )]]> <![CDATA[A w ]]> ZGO-550 5.903 393.1 0.00143 214.5 ZGO-650 2.813 148.5 0.00152 395.4 ZGO-750 14.75 632.4 0.00228 1240.5

[0053] The invention adopts a mixed solvent heat combined with high temperature calcination method to synthesize zinc germanate nanowires. The raw materials used in the method are low in cost, the method is simple to operate, the reaction conditions are relatively mild, the product has high purity, good crystallinity, uniform morphology, and its unit cell parameters are consistent with the standard atlas PDF#11-0687.

[0054] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0055] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. A method for preparing a zinc germanate material, characterized in that: The steps include: S1: Dissolve zinc acetate and germanium oxide in deionized water and ethylenediamine, stir the two solutions separately for 30 minutes until they are completely dissolved, and then mix and stir the two solutions for 15 minutes; S2: transferring the milky white solution obtained in S1) into a stainless steel reactor, placing the stainless steel reactor in an oven and heating it for a period of time, and then cooling it to room temperature; S3: washing the product obtained in S2) with distilled water and anhydrous ethanol respectively, centrifugally filtering, and vacuum drying after filtering; S4: The product obtained after vacuum drying in S3) is placed in an argon atmosphere and calcined at high temperature for a period of time to obtain the product zinc germanate nanowires.

2. The method for preparing a zinc germanate material according to claim 1, characterized in that: The zinc acetate in S1) has a molecular formula of Zn(Ac)2·2H2O, and a molar ratio of the zinc acetate to deionized water is 1.5:1-2.5:

1.

3. The method for preparing a zinc germanate material according to claim 1, characterized in that: The germanium oxide in S1) has a molecular formula of GeO2, and its molar ratio to ethylenediamine is 1.5:1-3:

1.

4. The method for preparing a zinc germanate material according to claim 1, characterized in that: The stainless steel reactor in S2) is placed in an oven and heated to 120-180° C., and the constant temperature reaction time is 3-36 hours.

5. The method for preparing a zinc germanate material according to claim 1, characterized in that: In the step S4), the vacuum dried product is placed in an argon atmosphere and calcined at a high temperature of 500-800° C. for 3-9 hours.

6. The method for preparing a zinc germanate material according to claim 5, characterized in that: When the calcination temperature is 650℃, the nanowire morphology is the most complete. When the temperature is too low, the reaction is incomplete. When the temperature is higher than 650℃, the nanowires agglomerate.

7. The zinc germanate nanowire material prepared by the method according to any one of claims 1 to 6.

8. The zinc germanate nanowire material according to claim 7, characterized in that: The charging platform of this material is around 1.0-1.2V, and when the current density is 100mAg -1 After 150 cycles of charge and discharge, the reversible specific capacity is stable at 1190 mAh g -1 , its impedance is small and the lithium ion diffusion coefficient is large; when the current density is 2000mAg -1 When the charge and discharge capacity is stable at 600mAh g -1 When the current density returns to 100mAg -1 When the charge-discharge capacity is 1000 mAh g -1 The rate performance is ideal.