Electronic-grade spherical titanium dioxide and preparation method thereof
Through the process flows such as acid dissolution, hydrolysis, precipitation, and roasting, combined with homemade complexing agents and dispersants, the problem of impurity contamination in the sulfuric acid method is solved, the purity and sphericality of titanium dioxide are improved, and it is suitable for high-end application fields and achieved Efficient purification and dispersion optimization.
Patent Information
- Application Number
- CN202411065394.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-05
AI Technical Summary
Among the existing titanium dioxide preparation methods, especially sulfuric acid, metal impurities are easily introduced, which affects the purity and performance of the product. Especially when purity is strictly required in high-end applications, the existing purification methods are complicated to operate and may introduce new impurities. The problem.
Using acid dissolution, hydrolysis, precipitation, roasting and other processes, by adding homemade complexing agents and dispersants, the metal impurities in metatitanic acid are removed, the purity of titanium dioxide is improved, and the agglomeration phenomenon is reduced through the dispersant in the hydrolysis stage, forming Titanium dioxide with excellent dispersion and high spherical shape.
It significantly improves the purity and sphericality of titanium dioxide, is suitable for high-end applications, reduces process costs and environmental pollution risks, and improves process efficiency.
Smart Images

Figure CN118929744A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of titanium dioxide, and in particular to electronic-grade spherical titanium dioxide and a preparation method thereof. Background Art
[0002] Titanium dioxide, due to its unique physical and chemical properties and excellent optical performance, has become an indispensable multifunctional material in modern industry. Its high refractive index, strong chemical stability, and non-toxicity make it widely used in traditional fields such as coatings, plastics, papermaking, rubber, and food additives. Furthermore, due to its high dielectric constant and resistivity, combined with its semiconductor properties, it also plays a key role in high-tech industries such as electronic ceramics, semiconductor capacitors, thermistors, and specialty glass.
[0003] Titanium dioxide is typically manufactured in either anatase or rutile crystal forms, with rutile being preferred in industrial applications due to its higher refractive index and improved weather resistance. In recent years, with the development of high-end manufacturing industries such as liquid crystal materials, precision sensors, and aerospace, market demand for high-purity titanium dioxide has continued to grow, and quality requirements have become increasingly stringent, particularly with regard to the control of impurities such as iron.
[0004] The preparation methods of titanium dioxide are mainly divided into gas phase method and liquid phase method. The gas phase method includes TiCl4 gas phase hydrogen flame hydrolysis method, TiCl4 gas phase oxidation method, titanium alkoxide gas phase hydrolysis method, etc. These methods can produce high-quality nano-scale titanium dioxide, but due to high equipment requirements, complex operation, high cost and other reasons, the scope of application is relatively small. The liquid phase method includes sulfuric acid method, hydrochloric acid method, sol-gel method, chloride liquid phase hydrolysis method, hydrothermal method, microemulsion method, etc. Compared with the gas phase method, the liquid phase method has lower equipment requirements, simple operation, wide source of raw materials, and low cost, so it has become a more common preparation method.
[0005] Currently, the industry primarily produces titanium dioxide using the vapor-phase TiCl₄ method, the liquid-phase sulfuric acid method, and the liquid-phase hydrolysis of titanium alkoxides. In China, the sulfuric acid method is the predominant production method. While this method offers advantages such as a simple and mature process, readily available raw materials, low cost, and simple equipment, it is prone to introducing impurities, which can affect product purity.
[0006] Metatitanic acid is a key intermediate in the sulfuric acid process for producing titanium dioxide. It is obtained by hydrolyzing titanyl sulfate after the reaction of ilmenite with sulfuric acid, followed by purification, freeze-drying to remove ferrous sulfate, filtration, and concentration. Metatitanic acid is not only a key raw material for titanium dioxide production but can also be used to prepare titanium-containing products such as nano-sized titanium dioxide, titanium sulfate, and titanyl sulfate.
[0007] However, due to differences in raw materials and production processes, unpurified metatitanic acid often contains significant amounts of metallic impurities, such as iron, magnesium, cobalt, manganese, chromium, niobium, sodium, or potassium. These impurities not only affect the hue of the final product but can also cause crystal lattice distortion, severely degrading product performance. For example, in the preparation of titanium dioxide, these impurities can cause the product's hue to shift yellow or red, reducing whiteness. In the preparation of nano-sized titanium dioxide, impurities can become crystal centers, leading to uneven particle size distribution and compromising its catalytic performance.
[0008] Therefore, the purification of metatitanic acid, especially the removal of metal impurities, becomes a key step in improving the quality of titanium dioxide.
[0009] Chinese patent document CN1613775A discloses a method for preparing rutile titanium dioxide electronic powder using metatitanic acid as the main raw material: (1) adding hydrochloric acid to metatitanic acid to adjust the acidity to pH ≤ 2.0, adding aluminum powder, zinc powder or iron powder as a powdered reducing agent to react, and the weight of the added reducing agent is 0.5-2% of the net weight of TiO2 in metatitanic acid; (2) adjusting the pH value of the material obtained after the treatment in step (1) to a pH value in the range of 2.0-4.0, and washing the above material with pure water; (3) adding 0.5-1.5% of a mixture of arsenic sulfide (realgar As4S4 or orpiment As2S3) and arsenic trioxide As2O3 to the material obtained in step (2) and stirring and mixing; (4) calcining the material obtained in step (3) at a temperature range of 820-960°C and keeping it at this temperature for 2.5-5 hours, and then allowing it to cool naturally to room temperature to obtain the finished product.
[0010] Current purification methods primarily include washing, bleaching, and salt treatment, but these methods are cumbersome and can introduce new impurities. To meet the stringent purity requirements of titanium dioxide for high-end applications, developing more efficient metatitanic acid purification methods has become a research priority. Summary of the Invention
[0011] In order to address the deficiencies in the prior art, the present invention aims to provide an electronic-grade spherical titanium dioxide and a preparation method thereof. Industrial metatitanic acid powder is used as raw material, and high-quality titanium dioxide products are prepared through a process of acidolysis, hydrolysis, precipitation, and roasting. The addition of a homemade chelating agent successfully removes metal impurities in metatitanic acid, significantly improving the purity of the final titanium dioxide product. The homemade dispersant introduced during the hydrolysis stage effectively reduces agglomeration, laying the foundation for the subsequent preparation of titanium dioxide with excellent dispersibility and high sphericity.
[0012] In order to achieve the above object, the present invention adopts the following technical solutions:
[0013] A method for preparing electronic-grade spherical titanium dioxide comprises the following steps:
[0014] (1) adding industrial metatitanic acid powder to a sulfuric acid solution, then adding a surfactant and a complexing agent, heating the mixture to react, obtaining an acid solution, filtering the acid solution, and diluting the acid solution to obtain a titanyl sulfate solution;
[0015] (2) adding a dispersant to the titanyl sulfate solution, hydrolyzing the solution, and then heat-insulating and aging the solution to obtain a titanium dioxide slurry;
[0016] (3) filtering and washing the titanium dioxide slurry, adjusting the pH, stirring and aging, adding ammonium sulfate, filtering and drying the product to obtain a powder;
[0017] (4) calcining, cooling, and grinding the powder obtained in step (3) to obtain the electronic grade spherical titanium dioxide.
[0018] Preferably, in step (1), the concentration of the sulfuric acid solution is 85-98 wt%; the dosage ratio of industrial metatitanic acid powder to sulfuric acid solution is 1 g: 2-10 mL; the dosage of the surfactant and the complexing agent are 0.5-2 wt% and 0.01-0.5 wt% of the industrial metatitanic acid powder, respectively.
[0019] Preferably, in step (1), the surfactant is one or more of an anionic surfactant and a nonionic surfactant; the heating reaction conditions are 90-150° C. for 1-6 hours; after the reaction is completed, the acid solution is diluted with deionized water to obtain a titanyl sulfate solution with a concentration of 200-500 g / L.
[0020] Preferably, in step (1), the structural formula of the complexing agent is one of Formula I or Formula II:
[0021]
[0022] More preferably, in step (1), the structural formula of the complexing agent is as follows:
[0023]
[0024] Specifically, in step (1), the preparation method of the complexing agent comprises the following steps:
[0025] Iminodiacetic acid and potassium carbonate are added to tetrahydrofuran, and trimesoyl chloride is slowly added dropwise under ice bath conditions. The reaction is stirred under ice bath conditions, and the product is rotary evaporated to remove the solvent tetrahydrofuran. Ethyl acetate is then added for extraction and separation, and the product is rotary evaporated and recrystallized in ethyl acetate to obtain the complexing agent.
[0026] Preferably, the molar ratio of the iminodiacetic acid, potassium carbonate, and trimesoyl chloride is 1:2.5-4:2-3.1.
[0027] Preferably, the trimesoyl chloride is added dropwise over 30 to 90 minutes, and the stirring reaction condition is 0 to 5° C. for 1 to 6 hours.
[0028] Under ice bath conditions (0-5° C.), iminodiacetic acid and potassium carbonate are mixed in a tetrahydrofuran solvent, and then trimesoyl chloride is slowly added dropwise, and the reaction is continued with stirring in the ice bath. After the reaction is completed, the tetrahydrofuran solvent is removed by a rotary evaporator, and then the product is extracted and separated with ethyl acetate, and then the ethyl acetate is removed again by a rotary evaporator, and finally recrystallized with ethyl acetate to obtain the final product complexing agent.
[0029] The core of this reaction is the acylation reaction between the acyl chloride and the amino group to form the N-substituted amide. Trimesoyl chloride contains three acyl chloride groups, which react with the secondary amine group in iminodiacetic acid. This acylation reaction is performed in an ice bath to slow the reaction rate, thereby increasing product yield and reducing the occurrence of side reactions. Slowly adding trimesoyl chloride ensures a more thorough reaction and avoids localized overdosage that can lead to increased side reactions.
[0030] As an alkaline substance, potassium carbonate not only removes acidic impurities from the raw materials but also provides the alkaline environment required for the reaction, promoting the reaction. In this process, potassium carbonate neutralizes by-products such as hydrochloric acid produced during the reaction, ensuring that the reaction medium remains alkaline.
[0031] In the post-processing step after the reaction is completed, the tetrahydrofuran solvent is removed by rotary evaporation (rotary evaporation) to obtain a preliminary product. Subsequently, the reaction mixture is extracted with ethyl acetate to separate non-polar impurities, and the ethyl acetate is then removed by rotary evaporation to obtain the refined product required for recrystallization. Finally, the product is further purified by recrystallization from ethyl acetate to ensure that the final complexing agent has a high purity.
[0032] Preferably, in step (2), the ratio of the dispersant to the titanyl sulfate solution is 0.1-3 g:100 mL.
[0033] Preferably, in step (2), the conditions for the hydrolysis reaction are hydrothermal reaction at 90-130° C. and 0.2-1 MPa for 2-12 h, and thermal aging for 1-3 h.
[0034] Preferably, in step (2), the structural formula of the dispersant is as follows:
[0035]
[0036] Specifically, in step (2), the preparation method of the dispersant comprises the following steps:
[0037] a. Dissolving polysuccinimide in DMSO to obtain a PSI solution; dissolving dopamine hydrochloride in DMSO, then adding triethylamine and ultrasonically oscillating to obtain a dopamine solution; adding the dopamine solution to the PSI solution, and refluxing under a nitrogen atmosphere to obtain a PSI-DA intermediate reaction solution;
[0038] b. dissolving glutamic acid in DMSO, then adding triethylamine and ultrasonically oscillating to obtain a glutamic acid solution; adding the glutamic acid solution to the intermediate reaction solution, stirring the reaction under a nitrogen atmosphere, adjusting the pH with an aqueous sodium hydroxide solution, precipitating the product with acetone, filtering, washing with acetone, and drying to obtain the dispersant.
[0039] Preferably, in step a, the ratio of PSI, dopamine hydrochloride, and triethylamine is 40 mmol: 10-15 mmol: 8-16 mL; the ultrasonic oscillation time is 10-30 min; and the reflux reaction conditions are reflux reaction at 50-70° C. for 18-30 h.
[0040] Preferably, in step b, the ratio of glutamic acid to triethylamine is 30 mmol:10-20 mL; the stirring reaction conditions are 50-70° C. for 12-20 h, and the pH is adjusted to 7-8 after the reaction is completed.
[0041] Preferably, the molar ratio of polysuccinimide, dopamine hydrochloride and glutamic acid is 40:10-15:30-25.
[0042] The reaction consists of two main steps, first the reaction of polysuccinimide (PSI) with dopamine (DA), and then the reaction of the PSI-DA intermediate with glutamic acid. In the first step, triethylamine acts as a strong base to neutralize dopamine hydrochloride, releasing free dopamine. The primary amine group (-NH2) of dopamine then undergoes nucleophilic addition to the imide ring of PSI. This process involves the nitrogen atom of the amino group attacking the carbonyl carbon of the imide ring to form a tetrahedral intermediate, which then collapses, leading to the opening of the imide ring and ultimately grafting dopamine onto the polysuccinimide molecular chain.
[0043] In the second step, the α-amino group of glutamic acid undergoes a similar nucleophilic addition reaction to the remaining imide ring of PSI. This process is similar to the first step, also involving the amino group attacking the carbonyl carbon of the imide ring to form a tetrahedral intermediate. The intermediate collapses, the imide ring opens, and glutamic acid is grafted onto the polysuccinimide molecule.
[0044] The reaction results in the ring-opening of some of the imide rings on the PSI backbone by dopamine, introducing dopamine side chains. The remaining imide rings are then opened by glutamic acid, introducing glutamic acid side chains. The final product is a polymer containing both dopamine and glutamic acid side chains, with some unreacted imide rings potentially remaining on the backbone.
[0045] By introducing side chains with specific functions onto the PSI skeleton, an amphiphilic polymer with good dispersion properties was successfully synthesized. It also combined multiple action mechanisms such as electrostatic stabilization, steric stabilization and chemical adsorption to achieve an efficient and stable dispersion effect.
[0046] Preferably, in step (3), the pH of the system is adjusted to 8-10 with aqueous ammonia, and the mixture is stirred and aged for 2-5 hours. The mass ratio of titanium dioxide slurry to ammonium sulfate is 100:0.5-2.
[0047] Preferably, in step (4), the calcination is carried out at 500-1000° C. for 2-5 hours.
[0048] The present invention also claims protection for electronic-grade spherical titanium dioxide prepared by the preparation method.
[0049] Compared with the prior art, the present invention has the following beneficial effects:
[0050] 1) The present invention provides a method for preparing electronic-grade spherical titanium dioxide, which uses readily available industrial metatitanic acid powder as a raw material and is prepared through acidolysis, hydrolysis, precipitation, roasting and other processes. 50 50~100nm, TiO2≥99.9wt%, Si≤0.05wt%, Al≤0.005wt%, Ca≤0.005wt%, Nb≤0.005wt%, V≤0.005wt%, Fe≤0.0005wt%, Cl≤0.005wt%, BET=15~30m 2 / g; the addition of a surfactant during the acidolysis process can effectively prevent the agglomeration and sedimentation of titanic acid powder, solubilize the impurities therein, and improve the reaction efficiency of titanic acid with sulfuric acid and a chelating agent; the addition of a homemade chelating agent can effectively remove metal impurities in titanic acid and improve the quality of titanium dioxide products; the addition of a homemade dispersant during the hydrolysis process can reduce the agglomeration of titanic acid during hydrolysis, which is conducive to the subsequent formation of titanium dioxide with good dispersion and sphericity.
[0051] 2) The present invention provides a homemade complexing agent containing multiple carboxyl functional groups, which can selectively form stable complexes with impurity ions such as alkali metals and alkaline earth metals in industrial metatitanic acid, significantly improving the solubility of impurities in acidic solutions, and helping to efficiently separate impurities from industrial metatitanic acid to obtain purer titanium products; compared with traditional strong acid leaching processes, the use of this complexing agent can reduce the amount of acid used, reduce the risk of environmental pollution, and also play an important role in improving product quality and enhancing process efficiency.
[0052] 3) The present invention provides a self-made dispersant, whose glutamic acid side chain contains a large number of carboxylic acid groups, which form carboxylates under alkaline conditions, causing the surface of the metatitanic acid colloidal particles formed after the hydrolysis of titanyl sulfate to be negatively charged, generating electrostatic repulsion, effectively preventing the particles from approaching and aggregating, and improving dispersion stability; in addition, the π bond of the dopamine side chain can form a coordination bond with the d-vacant orbital of the metal atom, so that the dopamine side chain is firmly adsorbed on the surface of the metatitanic acid colloidal particles. When the amide group in the dopamine side chain is close to the π bond, a larger π bond system is formed due to the conjugation effect, which significantly enhances the adsorption force of the derivative on the metal atom, thereby firmly anchoring the derivative on the surface of the metatitanic acid particles, preventing the loss of the dispersant, and maintaining a stable and long-lasting dispersion effect; finally, the spatial structure of the polymer main chain and side chain forms a protective layer on the surface of the colloidal particles, further preventing the particles from aggregating through the steric barrier effect, so that the titanium dioxide finally obtained has excellent sphericity and dispersibility, and is suitable for high-end application fields. BRIEF DESCRIPTION OF THE DRAWINGS
[0053] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the following briefly introduces the drawings required for use in the embodiments. It should be understood that the following drawings only show schematic diagrams of certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other relevant drawings can be obtained based on these drawings without paying any creative work.
[0054] Figure 1 This is a SEM photograph of titanium dioxide prepared in Example 4 of the present invention. DETAILED DESCRIPTION
[0055] In order to make the purpose, technical solutions and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with the embodiments. Of course, the specific embodiments described here are only used to explain the present invention and are not used to limit the present invention.
[0056] Unless otherwise specified, the chemical reagents and materials in the present invention are purchased from commercial sources or synthesized from commercially purchased raw materials.
[0057] A method for preparing a complexing agent comprises the following steps:
[0058] 10 mmol of iminodiacetic acid and 4 mmol of potassium carbonate were added to 50 mL of tetrahydrofuran, and 3.1 mmol of trimesoyl chloride (dissolved in 10 mL of tetrahydrofuran in advance) was slowly added dropwise under ice bath conditions. The addition was completed over 90 minutes, and the mixture was stirred in an ice bath for 1 hour. The product was rotary evaporated to remove the solvent tetrahydrofuran, and then ethyl acetate was added for extraction and separation. The product was rotary evaporated and recrystallized in ethyl acetate to obtain the complexing agent.
[0059] A method for preparing a dispersant comprises the following steps:
[0060] a. Dissolve 40 mmol of polysuccinimide in 15 mL of DMSO to obtain a PSI solution; dissolve 15 mmol of dopamine hydrochloride in 15 mL of DMSO, then add 12 mL of triethylamine and ultrasonically vibrate for 30 minutes to obtain a dopamine solution; add the dopamine solution to the PSI solution, and reflux at 60°C under a nitrogen atmosphere for 26 hours to obtain a PSI-DA intermediate reaction solution;
[0061] b. Dissolve 25 mmol of glutamic acid in DMSO, then add 14 mL of triethylamine, and ultrasonically oscillate for 30 minutes to obtain a glutamic acid solution; add the glutamic acid solution to the intermediate reaction solution, stir and react at 60° C. under a nitrogen atmosphere for 16 hours, adjust the pH to 8 with an aqueous sodium hydroxide solution, precipitate the product with acetone, filter, wash with acetone, and dry to obtain the dispersant.
[0062] The present invention will be further described below with reference to specific examples.
[0063] Example 1
[0064] A method for preparing electronic-grade spherical titanium dioxide comprises the following steps:
[0065] (1) 100 g of industrial metatitanic acid powder was added to 1000 mL of 98 wt% sulfuric acid solution, followed by the addition of 2 g of a surfactant, sodium hexadecylsulfonate, and 0.5 g of a complexing agent. The mixture was heated at 150° C. for 1 h to obtain an acid solution. The acid solution was filtered and diluted with deionized water to obtain a titanyl sulfate solution with a concentration of 500 g / L (based on the mass of titanium dioxide).
[0066] (2) Add 30 g of dispersant to 1000 mL of titanyl sulfate solution, hydrothermally react at 130° C. and 1 MPa for 2 h, and then age at this temperature for 3 h to obtain titanium dioxide slurry;
[0067] (3) 100 g of titanium dioxide slurry was filtered and washed, and the pH of the system was adjusted to 10 with aqueous ammonia. After stirring and aging for 5 h, 2 g of ammonium sulfate was added, and the product was filtered and dried to obtain a powder;
[0068] (4) calcining the powder obtained in step (3) at 900° C. for 3 h, cooling, and grinding to obtain the electronic grade spherical titanium dioxide, D 50 89nm, TiO2≥99.9wt%.
[0069] Example 2
[0070] A method for preparing electronic-grade spherical titanium dioxide comprises the following steps:
[0071] (1) 100 g of industrial metatitanic acid powder was added to 1000 mL of 95 wt% sulfuric acid solution, followed by the addition of 1.5 g of a surfactant, sodium hexadecylsulfonate, and 0.4 g of a complexing agent. The mixture was heated at 130° C. for 2 h to obtain an acid solution. The acid solution was filtered and diluted with deionized water to obtain a titanyl sulfate solution with a concentration of 400 g / L (based on the mass of titanium dioxide).
[0072] (2) Add 25 g of dispersant to 1000 mL of titanyl sulfate solution, hydrothermally react at 120° C. and 0.8 MPa for 4 h, and then age for 2 h to obtain titanium dioxide slurry;
[0073] (3) 100 g of titanium dioxide slurry was filtered and washed, and the pH of the system was adjusted to 9 with ammonia water. After stirring and aging for 4 h, 1.5 g of ammonium sulfate was added, and the product was filtered and dried to obtain a powder;
[0074] (4) calcining the powder obtained in step (3) at 800° C. for 4 h, cooling, and grinding to obtain the electronic grade spherical titanium dioxide, D 50 75nm, TiO2≥99.9wt%.
[0075] Example 3
[0076] A method for preparing electronic-grade spherical titanium dioxide comprises the following steps:
[0077] (1) 100 g of industrial metatitanic acid powder was added to 1000 mL of 93 wt% sulfuric acid solution, followed by the addition of 1 g of a surfactant, sodium hexadecylsulfonate, and 0.3 g of a complexing agent. The mixture was heated at 120° C. for 3 h to obtain an acid solution. The acid solution was filtered and diluted with deionized water to obtain a titanyl sulfate solution with a concentration of 300 g / L (based on the mass of titanium dioxide).
[0078] (2) Add 20 g of dispersant to 1000 mL of titanyl sulfate solution, hydrothermally react at 110° C. and 0.6 MPa for 8 h, and then age for 2 h to obtain titanium dioxide slurry;
[0079] (3) 100 g of titanium dioxide slurry was filtered and washed, and the pH of the system was adjusted to 9 with ammonia water. After stirring and aging for 3 h, 1 g of ammonium sulfate was added, and the product was filtered and dried to obtain a powder;
[0080] (4) The powder obtained in step (3) was calcined at 700° C. for 4.5 h, cooled, and ground to obtain the electronic grade spherical titanium dioxide. 50 67nm, TiO2≥99.9wt%.
[0081] Example 4
[0082] A method for preparing electronic-grade spherical titanium dioxide comprises the following steps:
[0083] (1) 100 g of industrial metatitanic acid powder was added to 1000 mL of 90 wt% sulfuric acid solution, followed by the addition of 0.5 g of a surfactant, sodium hexadecylsulfonate, and 0.01 g of a complexing agent. The mixture was heated at 90° C. for 6 h to obtain an acid solution. The acid solution was filtered and diluted with deionized water to obtain a titanyl sulfate solution with a concentration of 200 g / L (based on the mass of titanium dioxide).
[0084] (2) Add 1 g of dispersant to 1000 mL of titanyl sulfate solution, hydrothermally react at 90°C and 0.2 MPa for 12 h, and then age at this temperature for 1 h to obtain titanium dioxide slurry;
[0085] (3) 100 g of titanium dioxide slurry was filtered and washed, and the pH of the system was adjusted to 8 with aqueous ammonia. After stirring and aging for 2 h, 0.5 g of ammonium sulfate was added, and the product was filtered and dried to obtain a powder;
[0086] (4) calcining the powder obtained in step (3) at 700° C. for 5 h, cooling, and grinding to obtain the electronic grade spherical titanium dioxide, D 50 73nm, TiO2≥99.9wt%.
[0087] Figure 1 This is a SEM photograph of the titanium dioxide prepared in Example 4.
[0088] The above description is only a preferred specific embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any technician familiar with the technical field, within the technical scope disclosed by the present invention, who makes equivalent replacements or changes based on the technical solution and inventive concept of the present invention, should be covered by the scope of protection of the present invention.
Claims
1. A method for preparing electronic grade spherical titanium dioxide, It is characterized in that The steps include: (1) adding industrial metatitanic acid powder to a sulfuric acid solution, then adding a surfactant and a complexing agent, heating to react, obtaining an acid hydrolyzate, filtering and diluting the acid hydrolyzate to obtain a titanyl sulfate solution; (2) adding a dispersant to a titanyl sulfate solution, performing a hydrolysis reaction, and obtaining a titanium dioxide slurry after heat preservation and aging; (3) filtering and washing the titanium dioxide slurry, adjusting the pH, stirring and aging, adding ammonium sulfate, filtering and drying the product to obtain a powder; (4) calcining, cooling and grinding the powder obtained in step (3) to obtain the electronic grade spherical titanium dioxide.
2. The preparation method according to claim 1, It is characterized in that In step (1), the concentration of the sulfuric acid solution is 85-98wt%; the dosage ratio of industrial metatitanic acid powder to sulfuric acid solution is 1g:2-10mL; the dosage of the surfactant and the complexing agent are 0.5-2wt% and 0.01-0.5wt% of the industrial metatitanic acid powder, respectively.
3. The preparation method according to claim 1, It is characterized in that In step (1), the surfactant is one or more of anionic surfactant and nonionic surfactant; the heating reaction condition is 90-150° C. for 1-6 hours; after the reaction, the acid hydrolyzate is diluted with deionized water to obtain a titanyl sulfate solution with a concentration of 200-500 g / L.
4. The preparation method according to claim 1, It is characterized in that In step (1), the structural formula of the complexing agent is one of Formula I or Formula II:
5. The preparation method according to claim 1, It is characterized in that In step (2), the dosage ratio of the dispersant to the titanyl sulfate solution is 0.1-3 g:100 mL.
6. The preparation method according to claim 1, It is characterized in that In step (2), the conditions for the hydrolysis reaction are hydrothermal reaction at 90-130° C. and 0.2-1 MPa for 2-12 h, and heat preservation and aging for 1-3 h.
7. The preparation method according to claim 1, It is characterized in that In step (2), the structural formula of the dispersant is as follows:
8. The preparation method according to claim 1, It is characterized in that In step (3), the pH value of the system is adjusted to 8-10 with aqueous ammonia, and the mixture is stirred and aged for 2-5 hours. The mass ratio of titanium dioxide slurry to ammonium sulfate is 100:0.5-2.
9. The preparation method according to claim 1, It is characterized in that In step (4), calcination is performed at 500-1000° C. for 2-5 hours.
10. Electronic grade spherical titanium dioxide prepared by the preparation method according to any one of claims 1 to 9.
Citation Information
Patent Citations
Preparation method of titanyl sulfate
CN104692455A
Dark blue and white color material water-based dispersing agent for ink-jet printing and preparation method and application
CN106189514A
Method of hydrothermal preparation of high-purity titanium dioxide from industrial metatitanic acid
CN110357153A
Method for preparing high-purity titanium dioxide from titanium-containing blast furnace slag
CN112047377A
Method for purifying and removing iron from industrial meta-titanic acid
CN114014355A