Preparation method of low-carbon niobium pentoxide for superconducting niobium cast ingot

Through the refined process design, including heating the fluoroniobic acid solution and sectioned ammonia precipitation, washing and multiple calcination, the carbon content in niobium pentoxide was successfully reduced, and the carbon content in the prior art was difficult to reduce. The problem of this has improved the purity and production efficiency of superconducting niobium materials.

CN118929753APending Publication Date: 2024-11-12NINGXIA ORIENT TANTALUM INDUSTRY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410864493.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-30
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The prior art is difficult to effectively reduce the carbon content in niobium pentoxide, which makes it difficult for the purity of superconducting niobium materials to reach below 10 ppm, affecting the performance and production efficiency of the radio frequency superconducting cavity.

Method used

Through the refined process design, including heating the fluoroniobic acid solution, passing ammonia gas into sections for precipitation, washing and multiple calcination, controlling the precipitation and calcination process of niobium hydroxide, and reducing the carbon content in niobium pentoxide.

Benefits of technology

The successful preparation of niobium pentoxide with a carbon content of less than or equal to 10ppm reduces the difficulty of preparing superconducting niobium ingots, improves production efficiency and purity, and meets the requirements of RF superconducting cavity for high-purity niobium materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118929753A_ABST
    Figure CN118929753A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of low-carbon niobium pentoxide for a superconducting niobium cast ingot, which adopts steam to heat a fluoroniobic acid solution, and realizes efficient and environment-friendly niobium pentoxide production by controlling steam pressure and heating time. In the preparation process, the fluoroniobic acid solution is heated to a specific temperature and maintained for a certain time, then filtering, washing and calcining are carried out, and finally high-purity niobium pentoxide is obtained. According to the method, the product quality is improved, the production cost is reduced, and a new feasible way is provided for industrial production of niobium pentoxide. Compared with a traditional method, the method has the advantages of being simple in process, convenient to operate, low in cost, environmentally friendly and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of niobium material processing, and in particular to a method for preparing low-carbon niobium pentoxide for superconducting niobium ingots. Background Art

[0002] Niobium pentoxide is a key raw material for the production of metallic niobium and its carbides, and has important applications in many fields such as electronics, medicine and superconducting technology.

[0003] In superconducting technology, especially in the manufacture of radio frequency superconducting cavities, extremely high purity requirements are placed on niobium materials. Currently, the internationally recognized standard for high-purity niobium materials for radio frequency superconducting cavities clearly states that the content of interstitial inclusion elements, especially carbon, must be controlled below 10ppm (parts per million). Using low-carbon niobium pentoxide as the raw material for ingot casting can effectively avoid the reaction between carbon and niobium during the smelting process of superconducting niobium ingots, reduce processes, reduce energy consumption, and improve yield.

[0004] As the main raw material for superconducting niobium ingots, the carbon content in niobium pentoxide directly affects the purity of the final product. Unfortunately, the carbon content in niobium pentoxide currently available on the market is generally high, about 30ppm, which has become a key factor restricting the quality of high-purity niobium materials.

[0005] Niobium pentoxide is the raw material for superconducting niobium ingots. It is melted under vacuum conditions. The carbon in niobium pentoxide is first combined with oxygen to be removed in the form of carbon monoxide gas. However, when the oxygen mass fraction is reduced, the excess carbon cannot be further removed and will form carbides with high melting points and difficult to decompose and remove with the niobium matrix. After the excessive carbon element reacts with niobium, it will remain in the grain boundary gaps of high-purity niobium materials. It is one of the main elements that affect the RRR value of superconducting niobium materials. At the same time, it will reduce the thermal conductivity of niobium in the liquid helium temperature zone, which is not conducive to the heat generated by the radio frequency surface in the cavity to be transferred to the outside. Therefore, in order to meet the requirements of superconducting use, it is necessary to further remove the carbon element in the niobium ingot, and the process is difficult and complicated.

[0006] When niobium pentoxide is prepared by traditional processes, the carbon element mainly comes from the organic extractants used in the extraction and separation process of tantalum and niobium. The use of these organic extractants in the production process and a certain proportion of water solubility are the main sources of carbon in niobium pentoxide. Although there are patented technologies and research on reducing the carbon content in niobium materials in the industry, these methods either involve multiple smelting or involve complex and difficult process steps and high energy consumption. In the Chinese patent CN201410789578.X "A method for preparing high-purity niobium ingots for radio frequency superconducting cavities", 3 to 7 vacuum electron beam melting is used. By controlling the specific electric energy, the RRR value and composition of the prepared niobium ingots meet the requirements of high-purity niobium ingots for radio frequency superconducting cavities, and the carbon element is reduced to less than 10ppm. In order to make C ≤ 10ppm, the Chinese patent CN202010224935.3 "Processing method of high-purity niobium materials with high RRR value and niobium materials for radio frequency superconducting cavities" needs to be achieved through vacuum annealing technology, which is complex in process, difficult to control, and has the disadvantages of high energy consumption.

[0007] In addition, Ren Junshuai and others from the Nonferrous Metals Research Institute also pointed out the technical challenges of reducing the carbon content in their paper, including the need to conduct high temperature (>2000℃) and high vacuum (<10 -2 It takes three smeltings to obtain high-purity niobium materials with C≤10, which has a long process flow, low production efficiency and high energy consumption.

[0008] Although these efforts can eventually reduce the carbon content below the standard, the efficiency and cost-effectiveness of the entire process still need to be improved. It is against this background that the present invention conducts in-depth research on the carbon removal technology of niobium pentoxide, aiming to reduce the carbon content in niobium pentoxide to below 10ppm through a more efficient and energy-saving method, thereby meeting the stringent requirements of radio frequency superconducting cavities for high-purity niobium materials and promoting technological progress in related fields. Summary of the invention

[0009] The purpose of the present invention is to provide a method for preparing low-carbon niobium pentoxide for superconducting niobium ingots. Specifically, the present invention aims to prepare niobium pentoxide with a carbon content of less than or equal to 10ppm through refined process design, aiming to meet the high purity requirements of superconducting niobium ingots for raw materials, reduce the difficulty of preparing superconducting niobium ingots, and improve their performance.

[0010] To achieve the above object, the present invention adopts the following technical solutions:

[0011] The present invention relates to a method for preparing low-carbon niobium pentoxide for superconducting niobium ingots, the method comprising the following steps:

[0012] Step (1) heating the fluoroniobic acid solution, the heating method is not limited to hydrothermal, electric heating, steam heating, etc., preferably steam heating, so that the temperature of the fluoroniobic acid solution is controlled at 70-80° C.;

[0013] Step (2) introducing ammonia into the fluoroniobate solution obtained in step (1) in stages, maintaining the stirring blade speed at 90-100 rpm, and precipitating to pH = 4-5 in the first stage. The ammonia introduction time is controlled at 2-4 hours, preferably 3 hours, and more preferably 4 hours, so that the overall temperature of the system is further increased to above 90° C. on the basis of 70-80° C. in step (1), so that part of the organic matter is volatilized;

[0014] Step (3) continuing to introduce ammonia into the solution obtained in step (2), maintaining the stirring blade speed at 90-100 rpm, precipitating to pH = 8-9, and obtaining niobium hydroxide slurry, wherein the ammonia introduction time is controlled at 4-5 hours, preferably 4 hours, and more preferably 5 hours;

[0015] Step (4) the niobium hydroxide slurry obtained in step (3) is allowed to stand for 1-2 hours, preferably 1 hour, more preferably 2 hours, to allow the niobium hydroxide slurry and the supernatant to separate into layers, the niobium hydroxide settles at the bottom, the supernatant containing part of the organic matter is placed on the upper layer, and 50-200 L of the supernatant is extracted, an equal amount of pure water is added to the reactor, the stirring paddle is turned on and stirred for 10-30 minutes, and then the stirring paddle is turned off, and the reaction is continued to stand for 1-2 hours, and then 50-200 L of the supernatant is extracted again;

[0016] Step (5) adding hot ammonia water and hot pure water to the niobium hydroxide slurry obtained in step (4), the hot ammonia water washing time is 0.5-1.5 hours, preferably 1.5 hours, the hot ammonia water washing temperature is 60-80° C., preferably 80° C., the weight percentage concentration of ammonia in the ammonia water is 1.5%-2%, preferably 2%, the hot pure water washing time is 0.5-1 hour, preferably 1 hour, the hot pure water washing is 70-80° C., preferably 80° C., and the niobium hydroxide filter cake is obtained after filtering and washing;

[0017] Step (6) drying the niobium hydroxide filter cake obtained in step (5) in an oil-heated vacuum oven or an electric oven at a drying temperature of 140-200° C. for a drying time of 20-48 hours;

[0018] Step (7) calcining the dried niobium hydroxide obtained in step (6) once or more than once to obtain niobium pentoxide, the calcination temperature is 850-1000° C., the calcination equipment is not limited to a muffle furnace, a rotary kiln, a push boat furnace, etc., and the calcination time is 4-24 hours;

[0019] Step (8) The niobium pentoxide obtained in step (7) is subjected to -60 mesh grinding and screening to obtain low-carbon niobium pentoxide.

[0020] ) The present invention relates to a method for preparing low-carbon niobium pentoxide for superconducting niobium ingots, the method comprising the following steps:

[0021] The fluoroniobic acid solution is added into the reaction kettle, and the fluoroniobic acid solution is heated by introducing steam to maintain the temperature at 70-80°C.

[0022] While maintaining the stirring blade speed at 90-100 rpm, ammonia is introduced into the heated fluoroniobic acid solution, and the pH value of the solution is first adjusted to 4-5. The ammonia introduction time at this stage is controlled to be 2-4 hours. Then, ammonia is continued to be introduced until the pH value reaches 8-9, at which time the introduction of ammonia is stopped. The ammonia introduction time at this stage is controlled to be 4-5 hours, thereby obtaining niobium hydroxide slurry.

[0023] Turn off the stirring paddle, let the niobium hydroxide slurry stand for 1-2 hours, and then extract the supernatant. Then add an equal amount of pure water to the reactor, turn on the stirring paddle again, stir for 10-30 minutes, turn it off again, let it stand for another 1-2 hours, and then extract the supernatant again.

[0024] The niobium hydroxide is filtered and washed with hot ammonia water and hot pure water to obtain a niobium hydroxide filter cake.

[0025] The niobium hydroxide filter cake is placed in a drying oven at a temperature of 140-200° C. to dry to obtain dry niobium hydroxide.

[0026] The dried niobium hydroxide is calcined once or twice and then ground and sieved to finally obtain low-carbon niobium pentoxide, wherein the carbon content is ≤10ppm.

[0027] Compared with the existing niobium oxide production technology, the present invention has the following significant advantages:

[0028] 1. By effectively removing the carbon element from niobium pentoxide for superconducting niobium ingots, niobium pentoxide with a carbon content less than or equal to 10ppm was successfully prepared, which significantly reduced the carbon content of superconducting niobium ingots, thereby reducing the subsequent processing difficulty of superconducting niobium materials and improving the yield and production efficiency.

[0029] 2. By precisely controlling the temperature of the fluoroniobate solution system and the introduction rate of the precipitant, the present invention achieves effective crystal growth and reduction of specific surface area, reduces organic adhesion introduced during the extraction process, and efficiently prepares low-carbon niobium pentoxide.

[0030] 3. The precipitation technology of the present invention increases the grain size of niobium hydroxide, reduces the dispersibility of the system, and facilitates sedimentation, laying the foundation for multi-step residual organic separation technology, effectively removing aged organic matter floating on the surface of niobium hydroxide slurry, and further reducing the carbon impurity content.

[0031] 4. The process for preparing low-carbon niobium pentoxide according to the present invention is short and highly controllable, and has high industrial production application value.

[0032] Low-carbon niobium pentoxide is used as a raw material for niobium ingots for superconductivity. The reduction of its carbon content controls the carbon content in the superconducting niobium ingot from the source. The method of the present invention can reduce the subsequent use of repeated smelting and other methods to remove the carbon content in the niobium ingots for superconductivity, improve production efficiency, and reduce energy consumption during repeated smelting. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 The present invention is a process flow chart of a method for preparing low-carbon niobium pentoxide for superconducting niobium ingots. DETAILED DESCRIPTION

[0034] Preferred embodiments of the present invention are given below in conjunction with the accompanying drawings to illustrate the technical solutions of the present invention in detail.

[0035] Embodiment 1:

[0036] like Figure 1 As shown, the present invention provides a method for preparing low-carbon niobium pentoxide for superconducting niobium ingots, and the specific steps are as follows:

[0037] (1) Initial preparation:

[0038] Add 1200L of fluoroniobic acid solution to the reactor and start the stirring paddle to ensure that its speed is stable at 92 rpm to optimize the mixing effect.

[0039] (2) Solution heating:

[0040] The fluoroniobate solution was heated by introducing steam, with the steam pressure controlled between 0.1 MPa and 0.3 MPa. The heating process lasted for 1.5 hours until the solution temperature reached a stable 71.4°C.

[0041] (3) Precipitation process:

[0042] Ammonia gas was introduced into the heated fluoroniobic acid solution, and the ammonia gas was introduced steadily in the initial stage until the pH value of the solution reached 4, which took 2.5 hours. Subsequently, ammonia gas was continued to be introduced but at a reduced rate until the pH value rose to 9, which took 4 hours, thereby completing the precipitation of niobium hydroxide.

[0043] (4) Standing and washing:

[0044] Turn off the stirring paddle, let the precipitated niobium hydroxide stand for 1 hour, and then extract part of the supernatant. Then add an equal amount of deionized water and turn on the stirring paddle again to stir for 30 minutes, let it stand again and extract the supernatant. Then, use 60-80℃ hot ammonia water and 70-80℃ hot pure water to wash the niobium hydroxide to ensure the removal of impurities.

[0045] (5) Drying and calcination:

[0046] After washing, the niobium hydroxide filter cake is placed in a drying oven and dried at 140° C. for 24 hours. Subsequently, the dried niobium hydroxide is calcined at a high temperature between 850° C. and 1000° C. to finally obtain niobium pentoxide.

[0047] (6) Post-processing:

[0048] After calcination, the niobium pentoxide is ground and screened to obtain a low-carbon niobium pentoxide product.

[0049] After the above steps, we successfully prepared low-carbon niobium pentoxide. The specific test results are shown in Table 1. Its carbon content is controlled below 10ppm, which meets the raw material requirements for superconducting niobium ingots.

[0050] Embodiment 2:

[0051] The steps of Example 2 are similar to those of Example 1, but some parameters are adjusted:

[0052] The heating process continued for 2.5 hours until the temperature reached 78.3°C.

[0053] The ammonia introduction time was adjusted to 3.5 hours and 5 hours respectively.

[0054] The drying temperature was increased to 200°C.

[0055] The calcination was performed twice, and the first calcination was followed by cooling to room temperature and then calcination was performed again.

[0056] These adjustments are intended to explore the effects of different process parameters on the quality of the final product. The specific test results are shown in Table 1.

[0057] Example 3

[0058] (1) Add 1200 L of fluoroniobic acid solution into the reactor and turn on the stirring paddle, with the stirring paddle speed controlled at 92 rpm.

[0059] (2) Steam is introduced into the fluoroniobate solution to heat it to 75.6° C., with a steam pressure of 0.1-0.3 MPa, and the steam is introduced for 2 hours.

[0060] (3) Ammonia gas is introduced into the fluoroniobate solution heated to 75.6° C., and the ammonia gas is introduced steadily until the pH value is 4. The ammonia gas is introduced for 3 hours. Ammonia gas is continued to be introduced into the solution while the ammonia gas introduction rate is reduced until the pH value is 9. The ammonia gas is introduced for 4 hours.

[0061] (4) Turn off the stirring blade, let the precipitated niobium hydroxide stand for 2 hours, extract 50-200L of supernatant, add an equal amount of deionized water, turn on the stirring blade, stir for 30 minutes, turn off the stirring blade, let stand for another 2 hours, and extract 50L-200L of supernatant again; put the niobium hydroxide slurry into a filter press, wash with 60-80°C hot ammonia water, the weight percentage concentration of ammonia in the ammonia water is 1.5%-2%, the washing time is 1.5 hours, and the hot ammonia water washing is stopped after 1.5 hours; add hot pure water to the filter press to continue washing, the pure water temperature is 70-80°C, the washing time is 1 hour, and the hot pure water washing is stopped after 1 hour, and squeeze to obtain a niobium hydroxide filter cake.

[0062] (5) placing the niobium hydroxide filter cake into an oil-heated vacuum drying oven at a drying temperature of 140° C. for 16 hours; calcining the niobium hydroxide to obtain niobium pentoxide at a calcination temperature of 850-1000° C.

[0063] (6) The calcined niobium pentoxide is cooled to room temperature and then calcined again at a calcination temperature of 850-1000° C. After calcination, it is ground and sieved to obtain low-carbon niobium pentoxide. The specific test results are shown in Table 1.

[0064] Comparative Example 1:

[0065] In order to verify the effectiveness of the present invention, we also conducted comparative experiments:

[0066] Initial preparation and precipitation:

[0067] Similarly, 1200L of fluoroniobic acid solution was added to the reactor and the stirring blade was started. However, in this comparative experiment, ammonia gas was directly introduced for precipitation until the pH value reached 8-9.

[0068] Washing and drying:

[0069] The niobium hydroxide is washed with hot ammonia water at 70-80° C. (the weight percentage concentration of ammonia in the ammonia water is 1.5%-2%) and hot pure water. Subsequently, the niobium hydroxide filter cake is dried at 100-110° C. for 48 hours.

[0070] Calcination and post-treatment:

[0071] The niobium hydroxide is calcined at 950°C for 3-6 hours and then ground and sieved.

[0072] The specific test results are shown in Table 1.

[0073] Table 1

[0074] Implementation method 1 Implementation Method 2 Comparative Example 1 C content (ppm) 9 6 26

[0075] Through comparative experiments, we can clearly see that the carbon content of niobium pentoxide obtained in Comparative Example 1 which does not adopt the method of the present invention is much higher than that of Example 1 and Example 2, thereby verifying the effectiveness of the method of the present invention in reducing the carbon content in niobium pentoxide.

[0076] The innovation of the present invention is as follows: ① Heating the fluoroniobic acid solution to a certain temperature, and the subsequent precipitation process releases heat through acid-base neutralization, which further increases the system temperature to above 90°C before precipitation is formed (i.e. before pH 5), so that a small amount of organic (MIBK) dissolved in the system during the extraction process can be partially volatilized, thereby reducing the carbon content; ② After heating and staged precipitation, there is still a small amount of organic in the niobium hydroxide slurry. Standing can make the niobium hydroxide slurry settle and stratify, and some of the remaining organic remains in the supernatant. Through multiple separations, the organic can be further removed, thereby reducing the carbon content. ③ Multiple calcination technology can further reduce the carbon content in niobium pentoxide on the basis of a carbon content of less than 10ppm.

Claims

1. A method for preparing low-carbon niobium pentoxide for superconducting niobium ingots, characterized in that: The following steps are involved: (1) heating the fluoroniobate solution to 70-80°C; (2) While stirring, introducing ammonia gas into the heated fluoroniobic acid solution, first adjusting the pH value of the solution to 4-5, and then continuing to introduce ammonia gas until the pH value reaches 8-9, to obtain niobium hydroxide slurry; (3) allowing the niobium hydroxide slurry to stand and extracting the supernatant, then adding pure water to stir and allowing it to stand again to extract the supernatant; (4) filtering and washing niobium hydroxide with hot ammonia water and hot pure water to obtain a niobium hydroxide filter cake; (5) drying the niobium hydroxide filter cake to obtain dry niobium hydroxide; (6) The dried niobium hydroxide is calcined and then ground and sieved to obtain low-carbon niobium pentoxide, wherein the carbon content is ≤10 ppm.

2. The preparation method according to claim 1, characterized in that: The heating of the fluoroniobate solution is achieved by introducing steam, and the steam pressure is controlled between 0.1Mpa and 0.3Mpa.

3. The preparation method according to claim 1 or 2, characterized in that: During the process of introducing ammonia, first introduce it quickly within 2-4 hours until the pH value reaches 4-5, and then reduce the introduction speed to make the pH value reach 8-9 within 4-5 hours.

4. The preparation method according to claim 1 or 2, characterized in that: The niobium hydroxide slurry is allowed to stand for 1-2 hours, and an equal amount of pure water is added to the supernatant after extraction for stirring.

5. The preparation method according to claim 1 or 2, characterized in that: The temperature of hot ammonia water is 60-80℃, and the temperature of hot pure water is 70-80℃.

6. The preparation method according to claim 1 or 2, characterized in that: The drying temperature of the niobium hydroxide filter cake is 140-200°C, and the drying time is 24 hours.

7. The preparation method according to claim 1 or 2, characterized in that: The calcination temperature is 850°C-1000°C.

8. Use of low carbon niobium pentoxide prepared by the method according to any preceding claim in the preparation of superconducting niobium ingots.