Preparation method of micro-nano manganous-manganic oxide material
Through the liquid phase precipitation and oxidation method, the particle size of trimanganese tetraoxide material is controlled, which solves the problem of difficult particle size control in the prior art, and improves the performance of the material and the adaptability of industrial production.
Patent Information
- Application Number
- CN202411218626.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-02
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing methods suitable for large-scale production of trimanganese tetraoxide materials cannot control the product particle size to a low level, resulting in insufficient abrasive and dispersible properties of the material.
By using liquid precipitation and oxidation method, the reaction system pH value is controlled within the range of 7-12, and manganese salt and sodium hydroxide solution are pumped to aging and Filtration to obtain micro-nano trimanganese tetraoxide material with particles ranging from 50-150 nm.
The particle size is controlled within the range of 50-150nm, which improves the wearability and dispersion of the material, reduces the impurity content, and is suitable for industrial production.
Smart Images

Figure CN118929760A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of manganese manganese tetroxide materials for soft magnetism, and in particular to a method for preparing micro-nano manganese manganese tetroxide materials. Background Art
[0002] Manganese tetraoxide (abbreviated as manganese tetraoxide or Mn3O4) is an important raw material for the production of manganese-zinc ferrite soft magnetic materials in the electronics industry. It is mixed with iron and zinc oxides in a certain ratio, molded and sintered to form a high-performance magnetic conductive material - soft ferrite. my country first used manganese carbonate as a raw material to produce soft ferrite, but because the manganese tetraoxide products produced by this process are prone to fine cracks, the current manufacturers of manganese tetraoxide materials mostly use manganese salt precipitation oxidation method and metal manganese suspension oxidation method, such as the methods disclosed in CN1252385A, CN1252386A, CN103058280A and other patents.
[0003] As the world's largest producer and supplier of manganese tetraoxide, China produces about 110,000 tons of manganese tetraoxide annually. With the advancement of electrification and electrification, the market demand for soft ferrites will further expand in the future. However, in the field of high-end soft magnetic materials, Japan's Tosoh Corporation is still the leader. By comparison, the primary particle size of domestic related products is about 200-500nm, while the primary particle size of Tosoh Corporation's manganese tetraoxide products is 50-150nm. We believe that this is the fundamental reason for the performance gap between the two parties in terms of material grindability and dispersibility.
[0004] At present, the liquid phase preparation methods of micro-nano materials mainly include hydrothermal method, sol-gel method, etc., but such methods are limited by manufacturing costs and are difficult to carry out industrial large-scale production. In the invention patent application with the publication number CN113603145A, entitled "A method for preparing micro-nano manganese tetraoxide from a manganese sulfate solution", the use of precipitation oxidation method to prepare micro-nano manganese tetraoxide is disclosed. Although this method is conducive to large-scale production, it can only obtain products with D50 < 2μm. It can be seen from the attached drawings 3, 5, and 7 of the specification that the minimum size is also above 200nm. In summary, a preparation method for micro-nano manganese tetraoxide material is urgently needed to solve this problem. Summary of the invention
[0005] The purpose of the present invention is to provide a method for preparing micro-nano manganese tetraoxide material to solve the problem that the existing method suitable for large-scale production of manganese tetraoxide material cannot control the product particle size at a low level.
[0006] To achieve the above object, the present invention provides the following technical solution: a method for preparing micro-nano manganese tetraoxide material, comprising the following specific steps:
[0007] S1: placing the reaction vessel in a water bath, adding a certain amount of bottom water to the reaction vessel, and simultaneously adding a certain amount of ammonium salt, surfactant and self-template agent, starting stirring and maintaining a certain speed, and waiting for the bottom water temperature to reach a set value;
[0008] After the temperature of S2 reaches the set value, a certain amount of manganese salt solution of a certain concentration is pumped into the reaction vessel through a peristaltic pump to maintain a certain feeding speed, and at the same time, a certain concentration of sodium hydroxide solution is pumped into the reaction vessel through another peristaltic pump. During the manganese salt feeding process, the pH value of the reaction system is maintained at 7-11;
[0009] After the addition of S3 manganese salt is completed, continue to pump in the alkaline solution to maintain the reaction system at a pH of 6-12 for aging;
[0010] S4: filtering the aged material, washing it with deionized water for several times, and finally filtering and drying it to obtain a micro-nano manganese tetraoxide material with a primary particle size of 50-150 nm.
[0011] Preferably, in step S1, the organic ammonium salt is ammonium sulfate and / or ammonium chloride, the surfactant is one or more of stearic acid, sodium dioctyl succinate sulfonate, and sodium dodecylbenzene sulfonate, and the self-templating agent is one or more of hexadecyltrimethylammonium bromide, anodized aluminum oxide, and polystyrene; in step S2, the manganese salt uses battery-grade high-purity manganese sulfate and / or manganese chloride.
[0012] Preferably, the concentration of the manganese salt solution is 0.2M-2M, the total addition amount is 300-1000ml, the bottom water is 100-500ml deionized water, the organic ammonium salt is 1-50g, the surfactant is 0.1-10g, and the self-template agent is 0.01-2g.
[0013] Preferably, in step S1, the stirring speed is 300-700 rpm, and the bottom water temperature is set to 40-80°C.
[0014] Preferably, in step S2, the feeding rate of the manganese salt solution is 1-10 ml / min, and the concentration of the sodium hydroxide solution used is 1M-5M.
[0015] Preferably, in step S3, the aging time is 0.5h-15h.
[0016] Preferably, in step S4, the drying temperature is 60-180° C. and the drying time is 2 h-24 h.
[0017] Preferably, in step S4, the number of washing times is 1-5 times, and the amount of deionized water used is 1L-3L.
[0018] Compared with the prior art, the present invention has the following beneficial effects:
[0019] 1. The preparation method of the micro-nano manganese tetraoxide material adopts a liquid phase precipitation oxidation method, which is simple and easy to operate and easy to industrialize.
[0020] 2. The preparation method of the micro-nano manganese tetroxide material prepares the manganese tetroxide material while maintaining the reaction system at a relatively high pH value. The primary particle size of the prepared material is between 50-150 nm, and the grindability and dispersibility of the material are greatly improved on the existing basis. At the same time, it is also beneficial to overcome the fundamental problem of high impurity content faced by the manganese salt method in preparing the manganese tetroxide material. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 1 is a SEM image of manganese tetraoxide prepared in Example 1 of the present invention.
[0022] Figure 2 This is the SEM image of trimanganese tetraoxide prepared in Comparative Example 1. DETAILED DESCRIPTION
[0023] A method for preparing a micro-nano manganese tetraoxide material comprises the following specific steps:
[0024] S1: placing the reaction vessel in a water bath, adding a certain amount of bottom water to the reaction vessel, and simultaneously adding a certain amount of ammonium salt, surfactant and self-templating agent, starting stirring and maintaining a certain speed (e.g., 300-700 rpm), and waiting for the bottom water temperature to reach a set value, preferably 40-80°C;
[0025] After the temperature of S2 reaches the set value, a certain amount of manganese salt solution of a certain concentration is pumped into the reaction vessel through a peristaltic pump to maintain a certain feeding speed, and at the same time, a certain concentration of sodium hydroxide solution is pumped into the reaction vessel through another peristaltic pump. During the manganese salt feeding process, the pH value of the reaction system is maintained at 7-11;
[0026] After the addition of S3 manganese salt is completed, continue to pump in the alkaline solution to maintain the reaction system at a pH of 6-12 for aging, and the aging time can be 0.5h-15h;
[0027] S4: filtering the aged material, washing it with deionized water for several times, and finally filtering and drying it. The drying temperature can be set to 60-180° C., and the drying time can be 2h-24h to obtain a micro-nano manganese tetraoxide material with a primary particle size between 50-150nm.
[0028] For reference, in step S1, the organic ammonium salt is ammonium sulfate and / or ammonium chloride, the surfactant is one or more of stearic acid, sodium dioctyl succinate sulfonate, and sodium dodecylbenzene sulfonate, and the self-templating agent is one or more of hexadecyltrimethylammonium bromide, anodized aluminum oxide, and polystyrene; in step S2, the manganese salt uses battery-grade high-purity manganese sulfate and / or manganese chloride.
[0029] In a preferred embodiment, the concentration of the manganese salt solution is 0.2M-2M, the total addition amount is 300-1000ml, the base water is 100-500ml deionized water, the organic ammonium salt is 1-50g, the surfactant is 0.1-10g, and the self-template agent is 0.01-2g. The above values can be increased or decreased proportionally. For reference at this ratio, the washing times in step S4 can be 1-5 times, and the amount of deionized water used is 1L-3L.
[0030] In a preferred embodiment, the feeding rate of the manganese salt solution in step S2 can be 1-10 ml / min, and the concentration of the sodium hydroxide solution used can be selected from 1M to 5M.
[0031] Embodiment 1:
[0032] The reaction vessel was placed in a water bath, 300 ml of bottom water was added to the reaction vessel, and 30 g of ammonium sulfate, 1 g of dioctyl sodium sulfosuccinate and 0.1 g of hexadecyl trimethyl ammonium bromide were added simultaneously, stirring was started and the speed was maintained at 600 rpm, and after the bottom water reached 60°C; 400 ml of 1M manganese salt solution was pumped into the reaction vessel by a peristaltic pump at a feeding rate of 3 ml / min, and a 4M sodium hydroxide solution was pumped into the reaction vessel by another peristaltic pump to maintain the pH value of the reaction system in the range of 9.5-10; after the manganese salt addition process was completed, continuous stirring and continued pumping of sodium hydroxide solution to maintain the pH value of the reaction system in the range of 8-8.5 for aging for 12 hours; the obtained material was filtered, washed 3 times with 1 L of deionized water, filtered, and dried at 120°C for 12 hours to obtain a micro-nano manganese tetraoxide material, the SEM image of which is shown in FIG. Figure 1 The primary particle size of the product is between 50-150nm.
[0033] Embodiment 2:
[0034] The reaction vessel was placed in a water bath, 200 ml of bottom water was added to the reaction vessel, and 25 g of ammonium chloride, 1 g of stearic acid and 0.1 g of hexadecyltrimethylammonium bromide were added simultaneously, stirring was started and the rotation speed was maintained at 600 rpm. After the bottom water reached 70°C, 400 ml of 1 M manganese salt solution was pumped into the reaction vessel by a peristaltic pump at a feeding rate of 5 ml / min, and a 2 M sodium hydroxide solution was pumped into the reaction vessel by another peristaltic pump to maintain the pH value of the reaction system in the range of 9-9.5; after the manganese salt addition process was completed, stirring was continued and the sodium hydroxide solution was continued to be pumped in to maintain the pH value of the reaction system in the range of 8-8.5 for aging for 15 hours; the obtained material was filtered, washed 5 times with 1 L of deionized water, filtered, and dried at 160°C for 5 hours to obtain a micro-nano manganese tetraoxide material with primary particles between 50-150 nm.
[0035] Embodiment 3:
[0036] The reaction vessel was placed in a water bath, 300 ml of bottom water was added to the reaction vessel, and 15 g of ammonium sulfate + 20 g of ammonium chloride, 1 g of stearic acid and 1 g of anodized aluminum + 2 g of polystyrene were added simultaneously, stirring was started and the rotation speed was maintained at 500 rpm, and after the bottom water reached 70°C, 1000 ml of 0.5 M manganese salt solution was pumped into the reaction vessel by a peristaltic pump at a feeding rate of 10 ml / min, and a 1 M sodium hydroxide solution was pumped into the reaction vessel by another peristaltic pump to maintain the pH value of the reaction system in the range of 9-9.5; after the manganese salt feeding process was completed, stirring was continued and the sodium hydroxide solution was continued to be pumped in to maintain the pH value of the reaction system in the range of 7.5-8 for aging for 5 hours; the obtained material was filtered, and after washing 5 times with 1 L of deionized water, it was filtered and dried at 80°C for 24 hours to obtain a micro-nano manganese tetraoxide material with primary particles between 50-150 nm.
[0037] Comparative Example 1:
[0038] (1) 1 ton of electrolytic manganese flakes were added to a horizontal ball mill and wet-milled for 80 minutes to obtain a manganese slurry with a mesh size of less than 80;
[0039] (2) First 10m 3 Add 1m 3 deionized water, and then add 30 kg of ammonium chloride as a catalyst to the reactor, add the prepared manganese slurry to the reactor, and then add deionized water to the reactor to dilute the manganese slurry to obtain a reaction slurry with a mass percentage concentration of manganese of 30%, start the stirring impeller in the reactor, adjust the frequency converter, and set the stirring impeller speed to 200 r / min; at the same time, introduce air into the reactor and adjust the air flow rate to 100 m 3 / h,
[0040] (3) continuing the reaction until the pH value of the slurry drops to 6.5, thereby obtaining manganese tetraoxide slurry;
[0041] (4) Put the manganese tetraoxide slurry into a mixer, add deionized water and stir for 30 minutes, then wash and filter by vacuum filtration, and finally dry to obtain the manganese tetraoxide product.
[0042] The SEM image of the manganese tetraoxide product prepared in Comparative Example 1 is shown in Figure 2 , the primary particle size of the product is about 200-500nm.
[0043] The above are only preferred embodiments of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed by the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope defined by the claims.
[0044] The matters not described in detail in the present invention are all known technologies to those skilled in the art.
Claims
1. A method for preparing micro-nano manganese tetraoxide material, characterized in that: The specific steps include: S1: placing the reaction vessel in a water bath, adding a certain amount of bottom water to the reaction vessel, and simultaneously adding a certain amount of ammonium salt, surfactant and self-template agent, starting stirring and maintaining a certain speed, and waiting for the bottom water temperature to reach a set value; After the temperature of S2 reaches the set value, a certain amount of manganese salt solution of a certain concentration is pumped into the reaction vessel through a peristaltic pump to maintain a certain feeding speed, and at the same time, a certain concentration of sodium hydroxide solution is pumped into the reaction vessel through another peristaltic pump. During the manganese salt feeding process, the pH value of the reaction system is maintained at 7-11; After the addition of S3 manganese salt is completed, continue to pump in the alkaline solution to maintain the reaction system at a pH of 6-12 for aging; S4: filtering the aged material, washing it with deionized water for several times, and finally filtering and drying it to obtain a micro-nano manganese tetraoxide material with a primary particle size between 50-150 nm.
2. The method for preparing a micro-nano manganese tetraoxide material according to claim 1, characterized in that: In the step S1, the organic ammonium salt is ammonium sulfate and / or ammonium chloride, the surfactant is one or more of stearic acid, sodium dioctyl succinate sulfonate, and sodium dodecylbenzene sulfonate, and the self-templating agent is one or more of hexadecyltrimethylammonium bromide, anodized aluminum oxide, and polystyrene; in the step S2, the manganese salt uses battery-grade high-purity manganese sulfate and / or manganese chloride.
3. The method for preparing a micro-nano manganese tetraoxide material according to claim 2, characterized in that: The concentration of the manganese salt solution is 0.2M-2M, the total addition amount is 300-1000ml, the bottom water is 100-500ml deionized water, the organic ammonium salt is 1-50g, the surfactant is 0.1-10g, and the self-template agent is 0.01-2g.
4. The method for preparing a micro-nano manganese tetraoxide material according to claim 1, characterized in that: In the step S1, the stirring speed is 300-700 rpm, and the bottom water temperature is set to 40-80°C.
5. The method for preparing a micro-nano manganese tetraoxide material according to claim 1, characterized in that: In step S2, the feeding speed of the manganese salt solution is 1-10 ml / min, and the concentration of the sodium hydroxide solution used is 1M-5M.
6. The method for preparing a micro-nano manganese tetraoxide material according to claim 1, characterized in that: In step S3, the aging time is 0.5h-15h.
7. The method for preparing a micro-nano manganese tetraoxide material according to claim 1, characterized in that: In step S4, the drying temperature is 60-180° C. and the drying time is 2 h-24 h.
8. The method for preparing a micro-nano manganese tetraoxide material according to claim 3, characterized in that: In step S4, the washing times are 1-5 times, and the amount of deionized water used is 1L-3L.
Citation Information
Patent Citations
Method for preparing mangano-manganic oxide by liquid phase oxidation
CN103172117A
Synthesis method of cell-grade manganous-manganic oxide
CN110776015A
Method for preparing micro-nano manganous-manganic oxide from manganese sulfate solution
CN113603145A
Preparation method of manganous-manganic oxide material with controllable particle size for lithium manganate
CN115180651A
Preparation method of manganous-manganic oxide with high specific surface area and high dispersity and product of manganous-manganic oxide
CN115849452A