Method for preparing high-purity manganous-manganic oxide by using manganese chloride as raw material to perform precipitation oxidation and then performing water vapor calcination purification
By using manganese chloride, surfactant and catalyst in the preparation of trimanganese tetraoxide, combined with water vapor calcination technology, the problems of low purity and high impurities in the prior art are solved, and high purity is achieved. Low-cost preparation method, suitable for industrial production.
Patent Information
- Application Number
- CN202411311575.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-20
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-09-20
AI Technical Summary
In the prior art, trimanganese tetraoxide has low purity, high impurity content, high cost and high purity dependence on raw material, making it difficult to realize a preparation method with low cost, simple process and high purity.
Manganese chloride is used as raw material, and oxidizes the surfactant and catalyst are added, and then reacts with alkali liquid and passes into the oxidation gas. The mixed gas of water vapor and air is maintained during the calcination process to obtain high Pure trimanganese tetraoxide.
It improves the purity and particle size uniformity of trimanium tetraoxide, reduces impurity content, simplifies the process flow, is suitable for large-scale industrial production, and reduces the dependence on raw material purity and cost.
Smart Images

Figure CN118929761A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of chemical materials, and in particular to a method for preparing high-purity manganese tetraoxide. Background Art
[0002] Manganese tetraoxide (Mn3O4) is also known as black manganese ore in nature. Its theoretical manganese content is 72.03%. It is mainly used as a basic raw material in industries such as electronic products and new energy power batteries. Manganese tetraoxide products can be divided into electronic grade and battery grade. Electronic grade manganese tetraoxide is a key raw material for the production of manganese-zinc ferrite, which is mainly used in transformers, filters, inductors and other products; battery grade manganese tetraoxide is mainly used in lithium battery manganese positive electrode materials, including lithium manganate, lithium manganese iron phosphate and sodium ion battery layered oxides. In addition to the above main application areas, manganese tetraoxide can also be used in many fields such as petroleum weighting agents, pigments, resistors, etc.
[0003] CN109052480A discloses a manganese tetraoxide and a preparation method thereof. The method comprises the steps of mixing electrolytic manganese powder and water into a manganese slurry; adding an ammonium salt solution into the manganese slurry, stirring, and introducing an oxidizing gas to react to prepare the manganese tetraoxide. The method makes the manganese tetraoxide more difficult to obtain due to the high price of electrolytic manganese powder, and the purity of manganese powder has a greater impact on the manganese tetraoxide. Part of the impurities may be included in the stage of mixed oxidation to form the manganese tetraoxide, and there is no subsequent further impurity removal and purification process.
[0004] Therefore, how to further improve the purity of manganese tetraoxide, increase the manganese content, reduce impurities and reduce the dependence on the purity of raw materials and price fluctuations, so as to develop a synthesis method of manganese tetraoxide with low cost, simple process, easy access to raw materials and high purity is a problem that needs to be solved at present. Summary of the invention
[0005] In view of the problems existing in the above-mentioned prior art, the present invention provides a method for preparing high-purity manganese tetraoxide by precipitation oxidation of manganese chloride as a raw material and then calcining and purifying with water vapor. The specific scheme is as follows:
[0006] A method for preparing high-purity manganese tetraoxide by precipitating and oxidizing manganese chloride as a raw material and then calcining and purifying it with water vapor comprises the following steps:
[0007] Step 1, dissolving and mixing manganese chloride, a surfactant and a catalyst together;
[0008] Step 2, mixing the solution obtained in step 1 with the alkali solution in parallel and introducing an oxidizing gas to react;
[0009] Step 3, filtering the solution obtained in step 2, and drying the filter residue to obtain the primary product manganese tetraoxide;
[0010] Step 4: Grind the primary product obtained in step 3 and then calcine it in stages to obtain purified manganese tetraoxide;
[0011] The surfactant used in step 1 is EDTA-2Na; the catalyst is ammonium chloride; the alkali solution used in step 2 is sodium hydroxide solution; the oxidizing gas used in step 2 is air; and the atmosphere used for calcination in step 4 is a mixture of air and water vapor.
[0012] The amount of alkali solution added in step 2 is 200-300 mL. Preferably, the amount of alkali solution added in step 2 is 210-250 mL.
[0013] The reaction temperature in step 2 is 50-100° C. Preferably, the reaction temperature in step 2 is 70-90° C.
[0014] In step 2, air is used as the oxidizing gas.
[0015] The oxidation time in step 2 is 2-10 hours. Preferably, the oxidation time in step 2 is 4-8 hours.
[0016] The calcination process in step 4 is one-stage calcination: 500-600°C, 6-10h; two-stage calcination: 900-1000°C, 4-8h.
[0017] During the calcination process in step 4, a mixed gas of air and water vapor is continuously introduced.
[0018] The Mn content of the high-purity manganese tetraoxide prepared through purification is >71%.
[0019] The present invention has simple operation steps. Manganese chloride is mixed with a surfactant and a catalyst, mixed and stirred with liquid alkali in parallel, and air is introduced for oxidation to obtain the primary product trimanganese tetraoxide. Subsequently, high-temperature calcination is performed while a mixed gas of water vapor and air is introduced throughout the process to obtain the purified high-purity trimanganese tetraoxide. The method can obtain high-purity trimanganese tetraoxide with high purity, low impurity content and good dispersibility.
[0020] Compared with the prior art, the present invention has the following beneficial effects:
[0021] (1) The present invention adds a surfactant and a catalyst in the precipitation oxidation stage. When the alkali solution contacts and reacts with the manganese chloride solution, the morphology of the precipitated manganese hydroxide can be regulated, the agglomeration phenomenon can be reduced, and the manganese hydroxide precipitation can be oxidized more fully, so that the particle size of the prepared manganese tetraoxide is uniform, and the reaction is promoted, the reaction rate is increased, and the reaction time is reduced.
[0022] (2) The present invention uses two stages of high-temperature calcination in the purification stage, so that the raw materials such as manganese chloride and manganese hydroxide that have not reacted completely in the initial product are first converted into manganese oxide during the first stage of low-temperature calcination, thereby avoiding the melting of the raw materials that have not reacted yet, resulting in an incomplete reaction and a dangerous situation. The second stage of high-temperature calcination can further form trimanganese tetroxide and remove some impurities while shaping the trimanganese tetroxide.
[0023] (3) In the present invention, a mixed gas of water vapor and air is introduced throughout the calcination process. The oxygen in the air can help the substances that have not been converted into trimanganese tetraoxide to be converted into trimanganese tetraoxide. The water vapor can help to remove some impurities and reduce the occurrence of sublimation, so that the impurity content in trimanganese tetraoxide is reduced and the loss of trimanganese tetraoxide is reduced. The addition of water vapor can reduce the oxygen content in the mixed gas and avoid the excessive oxidation of trimanganese tetraoxide to form manganese oxides such as manganese dioxide during the calcination process, resulting in a decrease in manganese content and a decrease in the purity of trimanganese tetraoxide.
[0024] (4) The preparation process of the present invention is simple and easy to operate, and all conditions in the reaction process are controllable, which is suitable for large-scale industrial production.
[0025] (5) The Mn content in the high-purity manganese tetraoxide prepared by the present invention is higher than 71%. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 The figure shows a process flow diagram of the present invention for preparing trimanganese tetraoxide by precipitation oxidation step by step using manganese chloride as a raw material. DETAILED DESCRIPTION
[0027] In order to explain the present invention more clearly, the present invention is further described below in conjunction with the embodiments, but the scope of protection claimed is not limited to the description.
[0028] Comparative Example 1
[0029] Step 1: Add 214 g of manganese chloride tetrahydrate, 3.72 g of EDTA-2Na and 2 g of ammonium chloride into 1 L of water and stir thoroughly until completely dissolved.
[0030] Step 2: dilute 200 ml of 32% alkali solution to 1 L and add it to 2 L of water at a flow rate of 10 mL / min in parallel with the solution obtained in step 1. Stir and mix at 50°C at a speed of 300 rpm, and allow air to oxidize at a flow rate of 10 L / min for 2 h.
[0031] Step 3: Filter the solution obtained in step 2, and dry the filter residue to obtain the primary product manganese tetraoxide.
[0032] Comparative Example 2
[0033] Step 1: Add 214 g of manganese chloride tetrahydrate, 3.72 g of EDTA-2Na and 2 g of ammonium chloride into 1 L of water and stir thoroughly until completely dissolved.
[0034] Step 2: Dilute 220 ml of 32% alkali solution to 1 L and add it to 2 L of water at a flow rate of 10 mL / min. Stir and mix at 50°C at a speed of 300 rpm, and allow air to oxidize at a flow rate of 10 L / min for 2 h.
[0035] Step 3: Filter the solution obtained in step 2, and dry the filter residue to obtain the primary product manganese tetraoxide.
[0036] Comparative Example 3
[0037] Step 1: Add 214 g of manganese chloride tetrahydrate, 3.72 g of EDTA-2Na and 2 g of ammonium chloride into 1 L of water and stir thoroughly until completely dissolved.
[0038] Step 2: Dilute 220 ml of 32% alkali solution to 1 L and add it to 2 L of water at a flow rate of 10 mL / min. Stir and mix at 50°C at a speed of 300 rpm, and allow air to oxidize at a flow rate of 10 L / min for 6 hours.
[0039] Step 3: Filter the solution obtained in step 2, and dry the filter residue to obtain the primary product manganese tetraoxide.
[0040] Comparative Example 4
[0041] Step 1: Add 214 g of manganese chloride tetrahydrate, 3.72 g of EDTA-2Na and 2 g of ammonium chloride into 1 L of water and stir thoroughly until completely dissolved.
[0042] Step 2: Dilute 220 ml of 32% alkali solution to 1 L and add it to 2 L of water at a flow rate of 10 mL / min. Stir and mix at 80°C at a speed of 300 rpm, and allow air to oxidize at a flow rate of 10 L / min for 6 hours.
[0043] Step 3: Filter the solution obtained in step 2, and dry the filter residue to obtain the primary product manganese tetraoxide.
[0044] Comparative Example 5
[0045] Step 1: Add 214 g of manganese chloride tetrahydrate, 3.72 g of EDTA-2Na and 2 g of ammonium chloride into 1 L of water and stir thoroughly until completely dissolved.
[0046] Step 2: Dilute 220 ml of 32% alkali solution to 1 L and add it to 2 L of water at a flow rate of 10 mL / min. Stir and mix at 80°C at a speed of 300 rpm, and allow air to oxidize at a flow rate of 10 L / min for 6 hours.
[0047] Step 3: Filter the solution obtained in step 2, and dry the filter residue to obtain the primary product manganese tetraoxide.
[0048] Step 4: Grind the primary product obtained in step 3 and calcine it, heat it to 550°C at a heating rate of 5°C / min and keep it for 8h, then continue to heat it to 950°C at a heating rate of 5°C / min and keep it for 6h, continue to let air in during the whole process, and then naturally cool it to room temperature to obtain purified manganese tetraoxide.
[0049] Example 1
[0050] Step 1: Add 214 g of manganese chloride tetrahydrate, 3.72 g of EDTA-2Na and 2 g of ammonium chloride into 1 L of water and stir thoroughly until completely dissolved.
[0051] Step 2: Dilute 220 ml of 32% alkali solution to 1 L and add it to 2 L of water at a flow rate of 10 mL / min. Stir and mix at 80°C at a speed of 300 rpm, and allow air to oxidize at a flow rate of 10 L / min for 6 hours.
[0052] Step 3: Filter the solution obtained in step 2, and dry the filter residue to obtain the primary product manganese tetraoxide.
[0053] Step 4: Grind the primary product obtained in step 3 and calcine it, heat it to 500°C at a heating rate of 5°C / min and keep it for 6 hours, then continue to heat it to 900°C at a heating rate of 5°C / min and keep it for 4 hours, continuously introduce a mixed gas of water vapor and air throughout the process, and then naturally cool it to room temperature to obtain purified manganese tetraoxide.
[0054] Example 2
[0055] Step 1: Add 214 g of manganese chloride tetrahydrate, 3.72 g of EDTA-2Na and 2 g of ammonium chloride into 1 L of water and stir thoroughly until completely dissolved.
[0056] Step 2: Dilute 220 ml of 32% alkali solution to 1 L and add it to 2 L of water at a flow rate of 10 mL / min. Stir and mix at 80°C at a speed of 300 rpm, and allow air to oxidize at a flow rate of 10 L / min for 6 hours.
[0057] Step 3: Filter the solution obtained in step 2, and dry the filter residue to obtain the primary product manganese tetraoxide.
[0058] Step 4: Grind the primary product obtained in step 3 and calcine it, heat it to 550°C at a heating rate of 5°C / min and keep it for 6 hours, then continue to heat it to 950°C at a heating rate of 5°C / min and keep it for 4 hours, continuously introduce a mixed gas of water vapor and air throughout the process, and then naturally cool it to room temperature to obtain purified manganese tetraoxide.
[0059] Example 3
[0060] Step 1: Add 214 g of manganese chloride tetrahydrate, 3.72 g of EDTA-2Na and 2 g of ammonium chloride into 1 L of water and stir thoroughly until completely dissolved.
[0061] Step 2: Dilute 220 ml of 32% alkali solution to 1 L and add it to 2 L of water at a flow rate of 10 mL / min. Stir and mix at 80°C at a speed of 300 rpm, and allow air to oxidize at a flow rate of 10 L / min for 6 hours.
[0062] Step 3: Filter the solution obtained in step 2, and dry the filter residue to obtain the primary product manganese tetraoxide.
[0063] Step 4: Grind the primary product obtained in step 3 and calcine it, heat it to 550°C at a heating rate of 5°C / min and keep it for 8 hours, then continue to heat it to 950°C at a heating rate of 5°C / min and keep it for 6 hours, continuously introduce a mixed gas of water vapor and air throughout the process, and then naturally cool it to room temperature to obtain purified manganese tetraoxide.
[0064] Example 4
[0065] Step 1: Add 214 g of manganese chloride tetrahydrate, 3.72 g of EDTA-2Na and 2 g of ammonium chloride into 1 L of water and stir thoroughly until completely dissolved.
[0066] Step 2: Dilute 220 ml of 32% alkali solution to 1 L and add it to 2 L of water at a flow rate of 10 mL / min. Stir and mix at 80°C at a speed of 300 rpm, and allow air to oxidize at a flow rate of 10 L / min for 6 hours.
[0067] Step 3: Filter the solution obtained in step 2, and dry the filter residue to obtain the primary product manganese tetraoxide.
[0068] Step 4: Grind the primary product obtained in step 3 and calcine it, heat it to 600°C at a heating rate of 5°C / min and keep it for 10 hours, then continue to heat it to 1000°C at a heating rate of 5°C / min and keep it for 8 hours, continuously introduce a mixed gas of water vapor and air throughout the process, and then naturally cool it to room temperature to obtain purified manganese tetraoxide.
[0069] The analysis and comparison of different experimental results are shown in Table 1.
[0070] Table 1 Analysis and comparison of different experimental results
[0071] experiment Mn / % Si / % Mg / % Cl / % <![CDATA[Bulk density / (g / cm 3 )]]> Comparative Example 1 68.72 0.0071 0.0052 0.091 0.77 Comparative Example 2 69.36 0.0068 0.0045 0.085 0.75 Comparative Example 3 70.11 0.0066 0.0046 0.080 0.71 Comparative Example 4 70.54 0.0065 0.0041 0.079 0.73 Comparative Example 5 70.92 0.0051 0.0032 0.067 0.68 Example 1 71.30 0.0037 0.0022 0.022 0.64 Example 2 71.48 0.0031 0.0018 0.016 0.63 Example 3 71.62 0.0026 0.0017 0.013 0.64 Example 4 71.41 0.0024 0.0017 0.011 0.62
[0072] As can be seen from the results in the above table, in Comparative Examples 1, 2, 3, and 4, the amount of alkali solution added, the reaction temperature, and the oxidation time all have an effect on the formation of trimanganese tetraoxide. A sufficient amount of alkali solution can ensure sufficient reaction with the raw materials and keep the pH of the system in an alkaline state. Increasing the reaction temperature and extending the oxidation time can fully oxidize manganese hydroxide to increase the manganese content of the product. In Comparative Examples 4 and 5, the manganese content of trimanganese tetraoxide after calcination is further increased, and the impurity content is slightly reduced, indicating that calcination has the effect of purifying and removing impurities on the product.
[0073] Compared with Comparative Example 1, water vapor is added as a mixed gas for calcination in Examples 1, 2, 3, and 4, and the calcination temperature and time are increased and prolonged. It can be found that the addition of water vapor further removes impurities and increases the manganese content, making the purity of trimanganese tetraoxide higher. Properly extending the calcination time and increasing the calcination temperature are conducive to the formation of trimanganese tetraoxide. Excessive temperature and calcination time may cause trimanganese tetraoxide to be over-oxidized, thereby reducing the manganese content. Therefore, the calcination procedure should be preferably within 500-600°C, 6-10h; 900-1000°C, 4-8h.
[0074] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing high-purity manganese tetraoxide by precipitating and oxidizing manganese chloride as a raw material and then calcining and purifying it with water vapor, characterized in that: The following steps are involved: Step 1, dissolving and mixing manganese chloride, a surfactant and a catalyst together; Step 2, mixing the solution obtained in step 1 with the alkali solution in parallel and introducing an oxidizing gas to react; Step 3, filtering the solution obtained in step 2, and drying the filter residue to obtain the primary product manganese tetraoxide; Step 4: Grind the primary product obtained in step 3 and then calcine it in stages to obtain purified manganese tetraoxide; The surfactant used in step 1 is EDTA-2Na; the catalyst is ammonium chloride; The alkali solution used in step 2 is sodium hydroxide solution; the atmosphere used for staged calcination in step 4 is a mixture of air and water vapor.
2. The method for preparing high-purity trimanganese tetraoxide by precipitating and oxidizing manganese chloride as a raw material and then purifying it by steam calcination according to claim 1, characterized in that: The reaction temperature of step 2 is 50-100°C.
3. The method for preparing high-purity trimanganese tetraoxide by precipitating and oxidizing manganese chloride as a raw material and then calcining with water vapor for purification according to claim 2, characterized in that: The reaction temperature of step 2 is 70-90°C.
4. The method for preparing high-purity trimanganese tetraoxide by precipitating and oxidizing manganese chloride as a raw material and then calcining with water vapor for purification according to claim 1, characterized in that: In the second step, air is used as the oxidizing gas.
5. The method for preparing high-purity trimanganese tetraoxide by precipitating and oxidizing manganese chloride as a raw material and then calcining with water vapor for purification according to claim 1, characterized in that: In the step 2, an oxidizing gas is introduced for oxidation for 2-10 hours.
6. The method for preparing high-purity trimanganese tetraoxide by precipitation oxidation of manganese chloride as a raw material and then calcination with water vapor for purification according to claim 5, characterized in that: In the step 2, an oxidizing gas is introduced for oxidation for 4-8 hours.
7. The method for preparing high-purity trimanganese tetraoxide by precipitating and oxidizing manganese chloride as a raw material and then purifying it by steam calcination according to claim 1, characterized in that: The staged calcination process of step 4 is as follows: the first stage calcination: 500-600°C, 6-10 h; the second stage calcination: 900-1000°C, 4-8 h.
8. The method for preparing high-purity trimanganese tetraoxide by precipitation oxidation of manganese chloride as a raw material and then calcination with water vapor for purification according to claim 1, characterized in that: During the staged calcination in step 4, a mixed gas of air and water vapor is continuously introduced.
Citation Information
Patent Citations
High-purity manganous-manganic oxide and preparation method thereof
CN109052480A
Technology for preparing high-purity manganous-manganic oxide with manganese sulfate solution
CN103466720A
Method for refining iron oxide, iron oxide thus obtained and use thereof
CN118369293A