Papermaking white mud lightweight concrete as well as preparation method and application thereof
By replacing cement with papermaking white mud particles and combining probiotic treatment, low-specific gravity and high-strength lightweight concrete for papermaking white mud is prepared, solving the pollution of papermaking white mud treatment and the carbon emission of traditional concrete, realizing resource recycling and Environmentally friendly effect.
Patent Information
- Application Number
- CN202411045316.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-12
AI Technical Summary
The existing papermaking white mud treatment methods lead to surface water and groundwater pollution. In the traditional concrete production process, cement consumes a lot of energy and produces a large amount of carbon dioxide. The concrete proportion is large, making it difficult to reduce cement use to reduce carbon emissions.
Use papermaking white mud particles to replace part of the cement, combine it with probiotic treatment and calcination to prepare light concrete, and prepare low specific gravity, high compressive strength and cracking strength light concrete through dry mixing and stirring process to reduce cement use and reduce environmental pollution.
The resource reuse of papermaking white mud has been realized, the manufacturing cost and carbon emissions of concrete have been reduced, the strength and durability of concrete have been improved, the requirements of national standards have been met, and the prospect of environmental protection and market-oriented application are provided.
Smart Images

Figure BDA0004973340510000111 
Figure HDA0004973340520000011 
Figure HDA0004973340520000012
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of waste recycling, and in particular relates to a papermaking white mud lightweight concrete and a preparation method and application thereof. Background Art
[0002] According to statistics, the total pulp production in China reached 81.77 million tons in 2021, and every ton of pulp produced can produce 0.5 to 0.65 tons of papermaking mud. At present, the treatment method of these papermaking muds is still simple stacking and landfilling. Long-term landfilling of papermaking mud will produce high-concentration alkaline waste liquid, leading to surface water and groundwater pollution, and will also change soil properties and cause land salinization. Therefore, extensive development, simple stacking and landfilling treatment methods are no longer suitable for my country's development policies and environmental protection requirements. How to develop and reuse a large amount of papermaking mud as a resource requires further in-depth research.
[0003] Cement is one of the main components of concrete. The production process of cement consumes a lot of energy and produces a lot of carbon dioxide. According to statistics from the Global Cement and Concrete Association (GCCA), carbon emissions from the cement production process account for about 7% of global emissions. Therefore, reducing the amount of cement used in concrete can effectively reduce carbon emissions. Moreover, concrete made from cement and sand and gravel has a large specific gravity. In the process of mixing cement, sand and gravel with water to prepare concrete, water is not easy to evaporate completely. Therefore, a certain amount of water reducer needs to be added to improve the water-cement ratio, strength and durability of concrete, and avoid the high hydration heat generated during the hydration reaction of concrete, which leads to cracks in concrete. Water reducers are mostly anionic surfactants, such as lignin sulfonates, naphthalene sulfonate formaldehyde polymers, etc. The addition of water reducers helps to disperse cement particles, reduce unit water consumption, and improve the fluidity of concrete mixtures. However, excessive use of water reducers will reduce the friction between aggregate particles in concrete, resulting in reduced concrete strength. Therefore, how to find materials that can replace cement, use less or no water reducers, and prepare high-strength and low-specific gravity concrete at the same time is the focus of current industry research. Summary of the invention
[0004] In view of this, the object of the present invention is to provide a papermaking white mud lightweight concrete and a preparation method and application thereof. The papermaking white mud lightweight concrete prepared by the present invention has the characteristics of low specific gravity, high compressive strength and splitting strength.
[0005] The present invention provides a papermaking white mud lightweight concrete, wherein each cubic meter of the papermaking white mud lightweight concrete comprises the following amounts of preparation raw materials:
[0006] Coarse aggregate 1m 3 , 350kg of gel material, 720kg of gravel, water;
[0007] The water-binder ratio is 0.31 to 0.37;
[0008] The gel material is composed of cement and papermaking white mud particles; the mass of the papermaking white mud particles accounts for 5-15% of the mass of the gel material;
[0009] The coarse aggregate consists of crushed stone and ceramsite; the volume of the crushed stone accounts for 10-30% of the volume of the coarse aggregate.
[0010] Preferably, the crushed stone has a particle size of 20 to 40 mm and a Mohs hardness of 6 to 8;
[0011] The particle size of the ceramsite is 5-15 mm; the specifications of the cement include 52.5R; and the particle size of the gravel is 3-5 mm.
[0012] Preferably, the method for preparing the papermaking white mud particles comprises the following steps:
[0013] Mixing papermaking white mud with water to obtain white mud slurry;
[0014] The white mud slurry is allowed to stand, and the upper layer of impurities is separated and removed to obtain the lower layer of white mud;
[0015] The lower layer of white mud is mixed with the probiotic stock solution and aged to obtain aged mud;
[0016] The aged mud is calcined and then screened to obtain the papermaking white mud particles.
[0017] Preferably, the probiotic stock solution comprises probiotics and water;
[0018] The mass concentration of probiotics in the probiotic stock solution is 10-30%;
[0019] The probiotics include Bacillus and / or Cellulophagus;
[0020] The dosage ratio of the lower layer white mud to the probiotic stock solution is 1g:0.1-0.12mL.
[0021] Preferably, the standing time is 1 to 3 days, and the temperature is room temperature 25±5°C;
[0022] The aging temperature is room temperature 25±5°C, and the aging time is 12 to 60 hours;
[0023] The calcination temperature is 500-1200° C. and the calcination time is 4-10 hours.
[0024] Preferably, the particle size of the papermaking white mud particles is ≤0.224 mm.
[0025] The present invention also provides a method for preparing the papermaking white mud lightweight concrete described in the above technical solution, comprising the following preparation steps:
[0026] dry-mixing the coarse aggregate, the gel material and the gravel to obtain a premix;
[0027] Mixing the premix with water and stirring to obtain concrete slurry;
[0028] The concrete slurry is shaped to obtain the papermaking white mud lightweight concrete.
[0029] Preferably, the dry mixing time is ≥10 min; and the stirring time is ≥2 h.
[0030] Preferably, the shaping temperature is room temperature 25±5°C, and the shaping time is ≥24h.
[0031] The present invention also provides the application of the papermaking white mud lightweight concrete described in the above technical solution or the papermaking white mud lightweight concrete prepared by the preparation method in the field of building materials.
[0032] The present invention provides a papermaking white mud lightweight concrete, wherein each cubic meter of the papermaking white mud lightweight concrete comprises the following raw materials in the following amounts: coarse aggregate 1m 3 , 350kg of gel material, 720kg of gravel, and water; the water-cement ratio is 0.31-0.37; the gel material is composed of cement and papermaking white mud particles; the mass of the papermaking white mud particles accounts for 5-15% of the mass of the gel material; the coarse aggregate is composed of crushed stone and ceramsite; the volume of the crushed stone accounts for 10-30% of the volume of the coarse aggregate.
[0033] The present invention adopts papermaking white mud particles to replace part of cement as gel material, and no water reducing agent is needed to be added. On the one hand, the amount of cement in concrete is reduced, which helps to reduce carbon emissions; on the other hand, the papermaking white mud is recycled and reused, its application range is expanded, and the manufacturing cost of concrete is reduced. In addition, no water reducing agent is used in the preparation raw materials of the papermaking white mud lightweight concrete provided by the present invention, which reduces the pollution to the environment and soil. Moreover, although the present invention reduces the amount of cement, it does not affect the performance of the papermaking white mud lightweight concrete. The papermaking white mud particles can be used as a water reducing agent to absorb excess water in the concrete, reduce the internal stress of the concrete, avoid cracking, and improve the strength and hardness of the concrete. The obtained papermaking white mud lightweight concrete has a low specific gravity. The results of the embodiment show that when the papermaking white mud doping ratio is 15%, the compressive strength, splitting strength and early cracking strength of the papermaking white mud lightweight concrete are the highest, and the early cracking resistance performance grade reaches L-IV level. Therefore, adding a certain amount of papermaking white mud particles helps to improve the density, strength and durability of concrete.
[0034] The present invention also provides a method for preparing the papermaking white mud lightweight concrete described in the above technical scheme, comprising the following preparation steps: dry mixing aggregate, gel material and gravel to obtain a premix; mixing the premix with water and stirring to obtain concrete slurry; shaping the concrete slurry to obtain the papermaking white mud lightweight concrete.
[0035] The preparation method provided by the present invention is stable and reliable, and the performance of the prepared papermaking white mud lightweight concrete fully meets the requirements of national standards and has high feasibility. The present invention uses papermaking white mud to prepare lightweight concrete, providing a new development path for the resource recycling of papermaking waste. The preparation method provided by the present invention is simple to operate, has a wide source of raw materials, is low in cost, is pollution-free, is not only beneficial to environmental protection, but also has excellent performance of the prepared papermaking white mud lightweight concrete, and has considerable market application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 This is a SEM image of the papermaking white mud lightweight concrete prepared in Example 6;
[0037] Figure 2 This is a graph of the compressive strength of the papermaking white mud lightweight concrete prepared in Examples 6 to 8;
[0038] Figure 3 This is a graph showing the splitting strength of the papermaking white mud lightweight concrete prepared in Examples 6 to 8. DETAILED DESCRIPTION
[0039] The present invention provides a papermaking white mud lightweight concrete, wherein each cubic meter of the papermaking white mud lightweight concrete comprises the following amounts of preparation raw materials:
[0040] Coarse aggregate 1m 3 , 350kg of gel material, 720kg of gravel, water;
[0041] The water-binder ratio is 0.31 to 0.37;
[0042] The gel material is composed of cement and papermaking white mud particles; the mass of the papermaking white mud particles accounts for 5-15% of the mass of the gel material;
[0043] The coarse aggregate consists of crushed stone and ceramsite; the volume of the crushed stone accounts for 10-30% of the volume of the coarse aggregate.
[0044] In the present invention, unless otherwise specified, the raw materials used in the present invention are preferably commercially available products.
[0045] In the present invention, the raw materials for preparing the papermaking white mud lightweight concrete include 1m3 of coarse aggregate. 3. In the present invention, the coarse aggregate is composed of crushed stone and ceramsite. In the present invention, the volume of the crushed stone preferably accounts for 10-30% of the volume of the coarse aggregate, and more preferably 15-25%. In the present invention, the volume of the coarse aggregate is equal to the volume of the papermaking white mud lightweight concrete. In the present invention, the ratio of the volume of the crushed stone to the volume of the coarse aggregate is called the crushed stone volume replacement rate, and the crushed stone volume replacement rate is preferably 10-30%. The crushed stone volume replacement rate is adopted in the present invention to facilitate single variable comparison in the examples and comparative examples. In a specific embodiment of the present invention, the mass of the crushed stone is preferably 0-333.29 kg, and is not 0; the mass of the ceramsite is preferably 389.60-556.56 kg.
[0046] In the present invention, the particle size of the crushed stone is preferably 20 to 40 mm, more preferably 25 to 35 mm. In the present invention, the Mohs hardness of the crushed stone is preferably 6 to 8, more preferably 6.5 to 7.5, and further preferably 7. In the present invention, the shape of the crushed stone is preferably non-angular and / or smooth. The crushed stone in the present invention plays a skeleton role in concrete, and forms a solid structure after combining with cement and sand; the size, shape and hardness of the crushed stone will affect the strength and durability of the concrete; suitable crushed stone specifications and grading can reduce the gaps between the skeletons, save cement, and improve the strength of the concrete. Crushed stone can enhance the strength of the concrete foundation and adjust the uneven settlement of the foundation.
[0047] In the present invention, the particle size of the ceramsite is preferably 5 to 15 mm, more preferably 8 to 12 mm. The ceramsite in the present invention is used as a filling material for papermaking white mud lightweight concrete, and has the characteristics of light weight, heat preservation, and sound absorption, and can effectively improve the strength, sound insulation effect, and thermal insulation performance of concrete. Ceramsite can reduce the weight of concrete and make the concrete more stable. Ceramsite also has a high porosity and water absorption. When added to concrete, it can form a uniform waterproof layer. This waterproof layer not only has a good waterproof effect, but also has good air permeability, which can effectively prevent moisture and mold growth in the concrete wall.
[0048] In the present invention, the raw materials for preparing the papermaking mud lightweight concrete include 350kg of gel material per cubic meter. In the present invention, the gel material is composed of cement and papermaking mud particles. In the present invention, the mass of the papermaking mud particles accounts for 5-15% of the mass of the gel material, more preferably 7-15%, and specifically preferably one or more of 5%, 10% and 15%. In the present invention, the ratio of the mass of the papermaking mud particles to the mass of the gel material is called the papermaking mud doping ratio, and the papermaking mud doping ratio is 5-15%. The papermaking mud doping ratio is adopted in the present invention, which is conducive to the single variable change and comparison of the embodiments and comparative examples. The present invention adopts papermaking mud particles to replace part of the cement, which reduces the amount of cement on the one hand; on the other hand, the papermaking mud particles contain alumina, which can be used as a water reducer to absorb excess water in the concrete. In addition, the papermaking mud particles also contain a small amount of papermaking fibers, which can improve the strength and hardness of the concrete and reduce the specific gravity of the concrete, thereby realizing resource recycling. In a specific embodiment of the present invention, the mass of the papermaking white mud particles is preferably 17.5 to 52.5 kg, and more preferably 24.5 to 52.5 kg.
[0049] In the present invention, the specification model of the cement preferably includes 52.5R. In the present invention, the particle size of the papermaking white mud particles is preferably ≤0.224 mm, more preferably ≤0.112 mm.
[0050] In the present invention, cement reacts with water to form a gel that firmly bonds the concrete raw materials into a whole, and forms a solid cement stone after drying, so that the concrete has a certain strength, hardness and durability. Cement and water are mixed and filled into the gaps between crushed stone and ceramsite, effectively preventing concrete from cracking and water seepage, and improving the concrete's anti-permeability, compression, tension and fatigue resistance. Before hardening, cement gives concrete good fluidity, plasticity and shrinkage, thereby ensuring the construction performance and engineering quality of concrete. The present invention uses papermaking white mud particles to replace part of the cement, which has the effects of reducing deadweight, improving concrete strength and hardness, and improving thermal insulation.
[0051] In the present invention, the method for preparing the papermaking white mud particles preferably comprises the following steps:
[0052] Mixing papermaking white mud with water to obtain white mud slurry;
[0053] The white mud slurry is allowed to stand, and the upper layer of impurities is separated and removed to obtain the lower layer of white mud;
[0054] The lower layer of white mud is mixed with the probiotic stock solution and aged to obtain aged mud;
[0055] The aged mud is calcined and then screened to obtain the papermaking white mud particles.
[0056] The present invention mixes papermaking white mud with water to obtain white mud slurry. In the present invention, the mass ratio of the papermaking white mud to water is preferably 1:0.4-0.6. In the present invention, the mixing is preferably stirred up and down, and the stirring time is ≥2h, so that the white mud and water can be mixed evenly, so that the impurities in the papermaking white mud are fully dispersed or dissolved in the water, which is conducive to separation and impurity removal.
[0057] After obtaining the white mud slurry, the present invention allows the white mud slurry to stand, separates and removes impurities in the upper layer, and obtains the lower layer of white mud. In the present invention, the standing time is preferably 1 to 3 days, more preferably 2 to 3 days. In the present invention, the standing temperature is preferably room temperature 25±5°C, more preferably 25°C. The present invention can fully separate and remove impurities in papermaking white mud, including fiber debris, bleaching substances, and organic pollutants, etc., by standing, and the obtained lower layer of white mud is purer, achieving harmless building materials.
[0058] After obtaining the lower layer of white mud, the present invention mixes the lower layer of white mud with a probiotic stock solution and ages the mixture to obtain aged mud.
[0059] In the present invention, the probiotic stock solution preferably includes probiotics and water. In the present invention, the water is preferably deionized water or pure water. In the present invention, the mass concentration of probiotics in the probiotic stock solution is preferably 10-30%, more preferably 20-30%. In the present invention, the probiotics preferably include Bacillus and / or cellulophagus. In the present invention, the mass ratio of Bacillus and cellulophagus in the probiotics is preferably 0-1:0-1, more preferably 1:1.
[0060] In the present invention, the method for preparing the probiotic stock solution preferably comprises the following steps: mixing probiotics, brown sugar and water, and culturing to obtain the probiotic stock solution.
[0061] In the present invention, the culture is preferably carried out in a sealed state and under standard atmospheric pressure. In the present invention, the culture temperature is preferably 25±0.5°C, the culture time is preferably 12 to 24 hours, and more preferably 24 hours. In the present invention, the mass ratio of probiotics, brown sugar and water in the probiotic stock solution is preferably 0 to 0.5:1:45 to 55, and is not 0, and more preferably 0.2 to 0.4:1:50.
[0062] In the present invention, the dosage ratio of the lower layer of white mud and the probiotic stock solution is preferably 1g: 0.1-0.12mL, more preferably 1g: 0.11-0.12mL. In the present invention, the aging temperature is preferably room temperature 25±5°C, more preferably 25°C, and the aging time is preferably 12-60h, more preferably 36-40h. The present invention mixes the lower layer of white mud with the probiotic stock solution for aging. The probiotic stock solution can effectively decompose the organic matter remaining in the papermaking white mud, and avoid the generation of dioxins and other pollutants during calcination. The papermaking white mud and the probiotic stock solution are aged and fermented, and the material mixing is more uniform and fine, and the gas generated by the fermentation can form a "bubbling stirring" effect, forming fine pores in the papermaking white mud. The calcined papermaking white mud particles have abundant pores, which can improve the thermal insulation and heat insulation properties of the concrete and reduce the specific gravity of the concrete. In addition, the Bacillus and cellulophagus in the probiotic concentrate can reduce the heavy metals in papermaking mud, making papermaking mud lightweight concrete more environmentally friendly.
[0063] After obtaining the aged mud, the present invention calcines the aged mud and then screens it to obtain the papermaking white mud particles.
[0064] In the present invention, the calcination is preferably carried out in a silicon-molybdenum resistance furnace. In the present invention, the calcination temperature is preferably 500-1200°C, more preferably 800-1200°C. In the present invention, the heating rate to the calcination temperature is preferably 1-2°C / min, more preferably 1.5-2°C / min. In the present invention, the calcination time is preferably 4-10h, more preferably 6-10h. In the present invention, the calcined papermaking white mud is preferably screened in a vibrating screen. In the present invention, the aperture of the vibrating screen is preferably ≤0.224mm, more preferably ≤0.15mm. The present invention calcines the aged papermaking white mud, and the papermaking white mud particles contain fiber debris, organic matter, and other components that can be decomposed by the probiotic stock solution, and a large number of pores are formed after calcination, which has the advantages of many pores and good thermal insulation effect.
[0065] In the present invention, the raw materials for preparing the papermaking white mud lightweight concrete include 720 kg of gravel per cubic meter. In the present invention, the particle size of the gravel is preferably 3 to 5 mm.
[0066] In the present invention, gravel is filled between crushed stone and ceramsite to increase the compactness of concrete, improve the compressive strength and impermeability of concrete, prevent concrete shrinkage and cracking, improve the stability and fluidity of concrete, and make concrete easier to mix and pour. Gravel can adjust the dryness and wetness of cement in concrete, prevent concrete from being too dry or too wet, and extend the service life of concrete.
[0067] In the present invention, the raw materials for preparing the papermaking white mud lightweight concrete also include water per cubic meter. In the present invention, the water is preferably industrial water. In the present invention, the water-cement ratio of the papermaking white mud lightweight concrete is 0.31 to 0.37, preferably 0.31 to 0.35. In the present invention, the water-cement ratio is the mass ratio of water to gel material. The present invention uses the water-cement ratio to limit the amount of gel material and water in the papermaking white mud lightweight concrete, which is convenient for single variable comparison in the embodiments and comparative examples.
[0068] The present invention also provides a method for preparing the papermaking white mud lightweight concrete described in the above technical solution, comprising the following preparation steps:
[0069] dry-mixing the coarse aggregate, the gel material and the gravel to obtain a premix;
[0070] Mixing the premix with water and stirring to obtain concrete slurry;
[0071] The concrete slurry is shaped to obtain the papermaking white mud lightweight concrete.
[0072] The invention dry-mixes coarse aggregate, gel material and gravel to obtain a premix.
[0073] In the present invention, the dry mixing is preferably carried out in a forced mixer. In the present invention, the dry mixing time is preferably ≥ 10 min, more preferably ≥ 30 min.
[0074] In the present invention, the ceramsite in the coarse aggregate is preferably immersed in water before dry mixing. In the present invention, the immersion time is preferably 3 to 5 hours. In the present invention, the immersed ceramsite is preferably air-dried under room temperature and light-shielded conditions until there is no water droplet on the surface of the ceramsite before use.
[0075] After obtaining the premix, the present invention mixes the premix with water and stirs to obtain concrete slurry.
[0076] In the present invention, the stirring is preferably carried out in a forced mixer. In the present invention, the stirring time is preferably ≥ 2 h, more preferably ≥ 3 h.
[0077] After obtaining the concrete slurry, the present invention shapes the concrete slurry to obtain the papermaking white mud lightweight concrete.
[0078] In the present invention, the shaping is preferably carried out in a plastic beam mold. In the present invention, the shaping temperature is preferably room temperature 25±5° C. In the present invention, the shaping time is preferably ≥24h.
[0079] In a specific embodiment of the present invention, the papermaking white mud lightweight concrete in the mold is preferably compacted by vibration, and after being placed at room temperature for 24 hours, the mold is removed to obtain the shaped papermaking white mud lightweight concrete.
[0080] After the shaping, the present invention preferably further comprises curing the shaped papermaking white mud lightweight concrete. In the present invention, the curing is preferably carried out in a standard curing room. In the present invention, the curing temperature is preferably 20±2°C, and the relative humidity is preferably ≥95%. In the present invention, the curing duration is preferably 7 days and 28 days, more preferably 28 days. The present invention places the shaped papermaking white mud lightweight concrete in a curing room filled with saturated steam or a mixture of steam and air to accelerate the hardening of the concrete in a higher temperature and humidity environment.
[0081] The present invention also provides the application of the papermaking white mud lightweight concrete described in the above technical solution or the papermaking white mud lightweight concrete prepared by the preparation method in the field of building materials.
[0082] The technical solution of the present invention is further described below through specific implementation methods. Those skilled in the art should understand that the embodiments are only used to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0083] Example 1
[0084] 200 g of Bacillus, 200 g of Cellulophagus and 1 kg of brown sugar were added into 30 kg of pure water, mixed evenly, and then cultured at 25° C., sealed and under standard atmospheric pressure for 24 hours to obtain a probiotic stock solution.
[0085] Weigh 52.5 kg of papermaking white mud, add 21 kg of water, mix and let stand at 25°C for 24 hours, separate and remove the upper water layer and impurities to obtain the lower layer of white mud.
[0086] 52.5 kg of the obtained lower layer white mud was mixed with 5.25 L of probiotic stock solution, and aged at 25° C. for 24 h to obtain aged mud.
[0087] The aged mud was sent to a silicon-molybdenum resistance furnace, and the heating rate was set at 2°C / min. After the temperature was raised to 800°C, it was calcined for 6 hours. After the calcined aged mud was naturally cooled to room temperature, it was sent to a vibrating screen to obtain papermaking white mud particles with a particle size of 0.106-0.15mm.
[0088] Example 2
[0089] The only difference from Example 1 is that the amount of probiotic stock solution added is 63 L.
[0090] Example 3
[0091] The only difference from Example 1 is that the heating rate is 1.5°C / min.
[0092] Example 4
[0093] The only difference from Example 1 is that the calcination temperature is 1000°C.
[0094] Example 5
[0095] The only difference from Example 1 is that the calcination temperature is 1200°C.
[0096] Example 6
[0097] Weigh 389.60 kg of ceramsite, immerse it in water for 3 hours, and then spread the ceramsite out to air-dry at room temperature under light-shielding conditions until there are no water droplets on the surface.
[0098] According to the volume of crushed stone accounting for 30% of the volume of aggregate, that is, the volume replacement rate of crushed stone is 30%, weigh 333.29kg of crushed stone;
[0099] According to the mass of papermaking white mud particles accounting for 15% of the mass of the gel material, that is, the papermaking white mud doping ratio is 15%, 52.5 kg of papermaking white mud particles obtained in Example 1 and 297.5 kg of cement with a specification model of 52.5R are weighed;
[0100] Then weigh 720 kg of gravel with a particle size of 3 to 5 mm, add the above materials and the air-dried ceramsite into a forced mixer, and dry mix for 120 seconds to obtain a premix.
[0101] According to the water-binder ratio of 0.31, 108.5 kg of water was added to the premix and stirred for 120 seconds to obtain concrete slurry.
[0102] The obtained concrete slurry was loaded into a 150×150×150mm standard test block mold, compacted by vibration, and placed at room temperature for 24 hours. The mold was then removed to obtain a papermaking white mud lightweight concrete standard test block.
[0103] The obtained papermaking white mud lightweight concrete standard test blocks were tested after being cured for 28 days at 20°C and a relative humidity of 95%.
[0104] According to the Chinese standard GB / T 50081-2019 "Standard for Test Methods for Physical and Mechanical Properties of Concrete", relative density, compressive strength, splitting strength and early crack resistance tests are carried out.
[0105] The test results after 28 days of curing are: relative density is 814kg / m 3 , compressive strength 6.3MPa, splitting strength 0.76MPa, early crack resistance 120mm 2 / m 2 .
[0106] Figure 1 This is the SEM image of the papermaking white mud lightweight concrete prepared in Example 6. Figure 1 It can be seen that: Figure 1 The needle-shaped particles are the papermaking white mud particles prepared in Example 1. The papermaking white mud particles are needle-shaped on the outside and are stacked in an orderly manner. They are embedded with expanded clay and gravel in the middle and contain abundant pores, which is beneficial to reducing the specific gravity of the papermaking white mud lightweight concrete and improving the thermal insulation performance.
[0107] When the papermaking white mud doping ratio in Example 6 is 15%, the content of large-sized hexagonal plate-like calcium hydroxide crystals is extremely small ( Figure 1 The position of the winning red circle), there are many pores in the papermaking mud lightweight concrete. The cement, papermaking mud particles and water are mixed to react with hydration to form a gel, which interweaves and bonds the crushed stone, ceramsite and sand to form a concrete structure. In cement concrete, the strength of the hexagonal plate-like crystals of calcium hydroxide is very low and the stability is extremely poor. It is the first component to be corroded in the concrete. Moreover, the hexagonal plate-like crystals of calcium hydroxide are mostly enriched at the interface where cement and stone contact, and form coarse grains, which leads to a decrease in the bonding strength of the concrete interface. It is the weakest link in the cement concrete material. In actual applications, the content and size of the hexagonal plate-like crystals of calcium hydroxide will be monitored to ensure the performance of the concrete.
[0108] Example 7
[0109] The difference from Example 6 is that the papermaking white mud mixing ratio is 10%, and the crushed stone volume replacement ratio is 30%. The test results after 28 days of curing are: relative density is 843kg / m 3 , compressive strength 6.0MPa, splitting strength 0.74MPa, early crack resistance 132mm 2 / m 2 .
[0110] Example 8
[0111] The difference from Example 6 is that the papermaking white mud mixing ratio is 5%, and the crushed stone volume replacement rate is 10%. The test results after curing for 28 days are: the relative density is 875kg / m 3 , compressive strength 5.8MPa, splitting strength 0.75MPa, early crack resistance 135mm 2 / m 2 .
[0112] Example 9
[0113] The difference from Example 6 is that the water-to-binder ratio is 0.35.
[0114] The test results after 28 days of curing are: relative density is 822kg / m 3, compressive strength 6.0MPa, splitting strength 0.72MPa, early crack resistance 135mm 2 / m 2 .
[0115] Example 10
[0116] The difference from Example 6 is that the water-to-binder ratio is 0.37.
[0117] The test results after 28 days of curing are: relative density is 831kg / m 3 , compressive strength 6.1MPa, splitting strength 0.71MPa, early crack resistance 140mm 2 / m 2 .
[0118] Embodiment 11
[0119] The differences from Example 6 are as follows: the water-binder ratio is 0.37, the papermaking white mud doping ratio is 5%, and the crushed stone volume replacement rate is 10%.
[0120] The test results after 28 days of curing are: relative density is 867kg / m 3 , compressive strength 6.2MPa, splitting strength 0.72MPa, early crack resistance 130mm 2 / m 2 .
[0121] Example 12
[0122] The difference from Example 6 is that the papermaking white mud particles prepared in Example 2 are used.
[0123] The test results after 28 days of curing are: relative density is 819kg / m 3 , compressive strength 6.2MPa, splitting strength 0.75MPa, early crack resistance 125mm 2 / m 2 .
[0124] Example 13
[0125] The difference from Example 6 is that the papermaking white mud particles prepared in Example 4 are used.
[0126] The test results after 28 days of curing are: relative density is 825kg / m 3 , compressive strength 6.0MPa, splitting strength 0.71MPa, early crack resistance 128mm 2 / m 2 .
[0127] Embodiment 14
[0128] The difference from Example 6 is that the papermaking white mud particles prepared in Example 5 are used.
[0129] The test results after 28 days of curing are: relative density is 831kg / m 3 , compressive strength 6.0MPa, splitting strength 0.70MPa, early crack resistance 130mm 2 / m 2 .
[0130] Comparative Example 1
[0131] The difference from Example 6 is that no papermaking white mud particles are added, and 52.5 kg of commercially available water reducing agent lignin sulfonate is added.
[0132] The test results after 28 days of curing are: relative density is 1142kg / m 3 , compressive strength 5.9MPa, splitting strength 0.61MPa, early crack resistance 134mm 2 / m 2 .
[0133] Comparative Example 2
[0134] The difference from Example 6 is that no papermaking white mud particles and water reducing agent are added, and the amount of cement used is 350 kg.
[0135] The test results after 28 days of curing are: relative density is 1258kg / m 3 , compressive strength 5.6MPa, splitting strength 0.58MPa, early crack resistance 140mm 2 / m 2 .
[0136] In the embodiments and comparative examples of the present invention, the water-binder ratio, the papermaking white mud mixing ratio and the crushed stone volume replacement rate are used as variables, and the papermaking white mud lightweight concrete is synthesized by a single variable orthogonal test method and tested. The raw material details and test results of the embodiments and comparative examples are shown in Table 1.
[0137] Table 1 Raw material details and test results of Examples 6 to 14 and Comparative Examples 1 to 2
[0138]
[0139] Note: Examples 1 to 14 and Comparative Examples 1 to 2 all contain 720 kg of gravel;
[0140] In Comparative Example 1, 52.5 kg of commercially available water reducing agent lignin sulfonate was added.
[0141] Figure 2 The compressive strength diagram of the papermaking white mud lightweight concrete prepared in Examples 6 to 8 is shown in Table 1 and Figure 2It can be seen that: with the increase of the papermaking white mud mixing ratio, the compressive strength and splitting strength of the papermaking white mud lightweight concrete increase, that is, the compressive strength and splitting strength of the papermaking white mud lightweight concrete with a papermaking white mud mixing ratio of 15% are higher than those with a papermaking white mud mixing ratio of 5%. This shows that adding an appropriate amount of papermaking white mud particles can improve the compressive strength and splitting strength of papermaking white mud lightweight concrete.
[0142] According to GB / T 50081-2019 "Standard for Test Methods for Physical and Mechanical Properties of Concrete", the total cracking area per unit area c is the early crack resistance. When 100≤c≤400mm 2 / m 2 , for L-IV level, when c<100mm 2 / m 2 , which is LV level. Figure 3 The anti-splitting strength diagram of the papermaking white mud lightweight concrete prepared in Examples 6 to 8 is shown in FIG. Figure 3 It can be seen from Table 1 that with the increase of papermaking white mud doping ratio, the splitting strength of papermaking white mud lightweight concrete increases, and the splitting strength of papermaking white mud lightweight concrete decreases with the increase of calcination temperature. When the papermaking white mud doping ratio is 15%, the splitting strength and early crack resistance of papermaking white mud lightweight concrete are optimal, and the crack resistance grade can reach L-IV.
[0143] With the increase of water-binder ratio, the compressive properties of papermaking white mud lightweight concrete first decrease and then increase, and the splitting strength and early crack resistance gradually decrease. When the water-binder ratio is 0.31, the papermaking white mud doping ratio is 15% and the crushed stone volume replacement rate is 30%, the comprehensive performance of papermaking white mud lightweight concrete is optimal.
[0144] Compared with Example 12, the dosage of probiotics increased, and the compressive properties, splitting strength and early crack resistance of papermaking white mud lightweight concrete all decreased, indicating that the dosage of probiotics should be appropriate, and too much will affect the performance of papermaking white mud lightweight concrete.
[0145] Compared with Example 13 and Example 14, when the papermaking white mud doping ratio is 10% and 15%, the higher the calcination temperature of the papermaking white mud particles, the less change in the compressive strength of the papermaking white mud lightweight concrete, but the lower the splitting strength; when the papermaking white mud doping ratio is 15% and the calcination temperature is 800°C, the obtained papermaking white mud lightweight concrete has the highest splitting strength.
[0146] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be regarded as the protection scope of the present invention.
Claims
1. A papermaking white mud lightweight concrete, It is characterized in that Each cubic meter of the papermaking white mud lightweight concrete includes the following amounts of raw materials: Coarse aggregate 1m 3 , 350kg of gel material, 720kg of gravel, water; The water-binder ratio is 0.31 to 0.37; The gel material is composed of cement and papermaking white mud particles; the mass of the papermaking white mud particles accounts for 5-15% of the mass of the gel material; The coarse aggregate consists of crushed stone and ceramsite; the volume of the crushed stone accounts for 10-30% of the volume of the coarse aggregate.
2. The papermaking white mud lightweight concrete according to claim 1, It is characterized in that The particle size of the crushed stone is 20 to 40 mm, and the Mohs hardness is 6 to 8; The particle size of the ceramsite is 5-15 mm; the specifications of the cement include 52.5R; and the particle size of the gravel is 3-5 mm.
3. The papermaking white mud lightweight concrete according to claim 1, It is characterized in that The preparation method of the papermaking white mud particles comprises the following steps: Mixing papermaking white mud with water to obtain white mud slurry; The white mud slurry is allowed to stand, and the upper layer of impurities is separated and removed to obtain the lower layer of white mud; The lower layer of white mud is mixed with the probiotic stock solution and aged to obtain aged mud; The aged mud is calcined and then screened to obtain the papermaking white mud particles.
4. The papermaking white mud lightweight concrete according to claim 3, It is characterized in that The probiotic stock solution comprises probiotics and water; The mass concentration of probiotics in the probiotic stock solution is 10-30%; The probiotics include Bacillus and / or Cellulophagus; The dosage ratio of the lower layer white mud to the probiotic stock solution is 1g:0.1-0.12mL.
5. The papermaking white mud lightweight concrete according to claim 3, It is characterized in that The standing time is 1 to 3 days, and the temperature is room temperature 25±5°C; The aging temperature is room temperature 25±5°C, and the aging time is 12 to 60 hours; The calcination temperature is 500-1200° C. and the calcination time is 4-10 hours.
6. The papermaking white mud lightweight concrete according to claim 1 or 3, It is characterized in that The particle size of the papermaking white mud particles is ≤0.224 mm.
7. The method for preparing the papermaking white mud lightweight concrete according to any one of claims 1 to 6, It is characterized in that The method comprises the following preparation steps: dry-mixing the coarse aggregate, the gel material and the gravel to obtain a premix; Mixing the premix with water and stirring to obtain concrete slurry; The concrete slurry is shaped to obtain the papermaking white mud lightweight concrete.
8. The preparation method according to claim 7, It is characterized in that The dry mixing time is ≥10min; the stirring time is ≥2h.
9. The preparation method according to claim 7, It is characterized in that The setting temperature is room temperature 25±5°C, and the setting time is ≥24h.
10. Use of the papermaking white mud lightweight concrete according to any one of claims 1 to 6 or the papermaking white mud lightweight concrete prepared by the preparation method according to any one of claims 7 to 9 in the field of construction materials.