Active carbon sequestration cold bonding coarse aggregate as well as preparation method and application thereof

By cold bonding and granulating the construction waste slurry powder, alkali-modified biochar and cement, active carbon-solid cold bonded coarse aggregate that can absorb CO2 in situ is prepared, which solves the high cost of CO2 capture in the prior art The problem of this problem has achieved low-cost and environmentally friendly CO2 absorption and storage, and improved the mechanical properties of the aggregate.

CN118930169APending Publication Date: 2024-11-12SHENZHEN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410992285.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing CO2 capture, adsorption and storage technologies are costly and require transportation, and cannot achieve in-situ absorption, affecting the carbon footprint of the construction industry.

Method used

Cold bonding and granulation are used to use construction waste slurry powder, alkali-modified biochar and cement to prepare active carbon-solid cold bonding coarse aggregate, which absorbs CO2 in situ, and reduces energy consumption through cold bonding granulation. .

Benefits of technology

It has achieved low-cost, in-situ CO2 absorption and storage, improved the mechanical properties and carbonization of aggregates, reduced environmental pollution and energy consumption, and promoted the resource utilization of construction waste.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930169A_ABST
    Figure CN118930169A_ABST
Patent Text Reader

Abstract

The invention discloses an active carbon sequestration cold bonding coarse aggregate and a preparation method and application thereof.The preparation method of the active carbon sequestration cold bonding coarse aggregate comprises the following steps that by mass, 90 parts of building waste slurry powder, 10 parts of cement and 0-15 parts of alkali modified biochar are mixed, and a mixture is obtained; no 0 part of alkali modified biochar is taken; carrying out cold bonding granulation on the mixture, and curing to obtain active carbon sequestration cold bonding coarse aggregate; wherein the building waste slurry powder is obtained by hardening building waste slurry and then carrying out ball milling; the alkali modified biochar is obtained by soaking biochar in an alkali metal hydroxide solution and then drying. The cost of the adopted raw materials is low, energy consumption can be reduced through cold bonding granulation, meanwhile, it can be guaranteed that the coarse aggregate has large porosity, it is guaranteed that CO2 can effectively enter the coarse aggregate, capture and storage of CO2 are achieved, and every 1 kg of coarse aggregate can absorb 100-180 g of CO2 in situ.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of building materials, and in particular to an active carbon-fixing cold-bonding coarse aggregate and a preparation method and application thereof. Background Art

[0002] Due to the rapid development of cities and economy, the greenhouse effect is becoming more and more serious. Carbon dioxide (CO2) is one of the most important greenhouse gases. Currently, CO2 capture, adsorption and storage (CCUS) is considered to be the most effective technology to reduce carbon dioxide.

[0003] However, because traditional ex-situ CO2 capture, adsorption and storage technologies need to collect and seal waste gas produced by factories and require transportation costs, it costs 600-1800 yuan to remove one ton of CO2 from the atmosphere. Aggregates are used in large quantities in the construction industry. Therefore, it would be of great significance to provide a low-cost aggregate that can absorb CO2 in situ to achieve CO2 capture and storage. Summary of the invention

[0004] Based on the above-mentioned deficiencies in the prior art, the purpose of the present invention is to provide an active carbon-fixing cold-bonded coarse aggregate and a preparation method and application thereof, aiming to provide an aggregate with low cost and capable of absorbing CO2 in situ.

[0005] The technical solution of the present invention is as follows:

[0006] A first aspect of the present invention provides a method for preparing an actively carbon-fixed cold-bonded coarse aggregate, comprising the following steps:

[0007] By weight, 90 parts of construction waste slurry powder, 10 parts of cement, and 0-15 parts of alkali-modified biochar are mixed to obtain a mixture; wherein the alkali-modified biochar is not taken as 0 part;

[0008] The mixture is subjected to cold bonding granulation and curing to obtain the active carbon-fixing cold bonding coarse aggregate;

[0009] The construction waste slurry powder is obtained by hardening the construction waste slurry and then ball milling it;

[0010] The alkali-modified biochar is obtained by soaking the biochar in an alkali metal hydroxide solution and then drying it.

[0011] Optionally, the particle size of the actively carbon-fixed cold-bonded coarse aggregate is greater than 4.75 mm.

[0012] Optionally, the cement is ordinary Portland cement.

[0013] Optionally, the preparation method of the alkali-modified biochar specifically comprises the following steps:

[0014] Step A, adding biochar powder to deionized water, stirring, standing, discarding the supernatant, and obtaining a precipitate;

[0015] Step B, adding an alkali metal hydroxide solution to the precipitate, stirring, allowing to stand, and discarding the supernatant to obtain a precipitate;

[0016] Step C, adding deionized water to the precipitate, stirring, standing, and discarding the supernatant to obtain a precipitate;

[0017] Step D, repeating step C several times, drying the obtained precipitate to obtain the alkali-modified biochar.

[0018] Optionally, the particle size of the biochar powder is less than 150 μm; the particle size of the construction waste slurry powder is less than 150 μm;

[0019] The alkali metal hydroxide solution includes at least one of a potassium hydroxide solution and a sodium hydroxide solution.

[0020] Optionally, the step of cold bonding and granulating the mixed material specifically comprises:

[0021] The mixed materials are fed into a disc granulator in batches for cold bonding granulation, and water is sprayed during the feeding process, with the total water consumption being 15% to 20% of the mass of the mixed materials.

[0022] Optionally, the parameters of the disc granulator are: disc inclination angle of 45 to 60°, disc diameter of 0.5 to 2 m, edge height of 15 to 20 cm, and rotation speed of 15 to 35 rpm.

[0023] Optionally, the curing conditions are: sealed water bath curing at a temperature of 20±2°C for at least 28 days; or, the curing conditions are: constant temperature and humidity curing at a temperature of 20±2°C, a humidity greater than 95%, for at least 28 days.

[0024] A second aspect of the present invention provides an actively carbon-fixed cold-bonded coarse aggregate, wherein the actively carbon-fixed cold-bonded coarse aggregate is prepared by the preparation method of the present invention as described above.

[0025] A third aspect of the present invention provides a carbon fixation method, wherein the actively carbon-fixing cold-bonded coarse aggregate as described above is placed in an environment to be carbon-fixed, and the actively carbon-fixing cold-bonded coarse aggregate is utilized to absorb carbon dioxide to perform carbon fixation.

[0026] Beneficial effects: The present invention uses relatively low-priced construction waste slurry powder as filler and main carrier for carbon fixation, biochar as carbon absorption material, cement as binder, and the raw material cost is relatively low; further, cold bonding granulation is used to effectively gather the raw materials to prepare active carbon fixation cold bonding coarse aggregate. Compared with other granulation technologies, cold bonding granulation can reduce energy consumption, reduce carbon dioxide generated in the production process, protect the environment, save natural resources, and at the same time ensure that the prepared coarse aggregate has a large porosity, ensuring that CO2 can effectively enter the interior of the aggregate, so that the construction waste slurry therein captures and seals CO2. The active carbon fixation cold bonding coarse aggregate prepared by the present invention can absorb 100 to 180 g of CO2 in situ per 1 kg of active carbon fixation cold bonding coarse aggregate. The mechanical properties of the active carbon fixation cold bonding coarse aggregate are significantly improved after carbonization. The crushing strength of a single particle will increase by 8% to 75% and remain between 2.5 and 5.5 MPa; the water absorption rate will remain between 11% and 14%; the apparent density will increase by 4% to 10% and remain at 1550 g / cm 3 ~1800g / cm 3 Between. Construction waste slurry will cause pollution to the land when it is landfilled. The present invention uses construction waste slurry powder as raw material, realizes the resource utilization of construction waste slurry, reduces the problems caused by treatment and landfill, and is also beneficial to the sustainable development of building materials. The shortage of natural stone and the energy consumption and environmental pollution that may be caused by mountain blasting during the mining of coarse aggregates, and the active carbon fixation cold bonding coarse aggregate provided by the present invention can be used instead of natural aggregate, reducing the damage to the environment caused by the mining of natural aggregates. The sale of the active carbon fixation cold bonding coarse aggregate can also bring economic benefits. In addition, due to the large demand for concrete, the demand for aggregates is also large, so the present invention can significantly increase the recycling of construction waste slurry. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 Schematic diagram of the granulation of active carbon fixation cold bonding coarse aggregate.

[0028] Figure 2 (a) is a physical picture of construction waste slurry powder, and (b) is a SEM picture of construction waste slurry powder.

[0029] Figure 3 (a) is a physical picture of biochar powder, and (b) is a SEM picture of biochar powder.

[0030] Figure 4 Schematic diagram of the preparation process of active carbon fixation cold bonding coarse aggregate.

[0031] Figure 5Graph showing particle size distribution of untreated biochar, alkali-modified biochar, construction waste slurry powder, and ordinary Portland cement in the examples.

[0032] Figure 6 The figures are the results of carbon fixation capacity test, wherein (a) is the cross-sectional result figure of the carbonized coarse aggregate after active carbon fixation and cold bonding in comparative example 1, (b) is the cross-sectional result figure of the carbonized coarse aggregate after active carbon fixation and cold bonding in comparative example 2, and (c) is the cross-sectional result figure of the carbonized coarse aggregate after active carbon fixation and cold bonding in embodiment 1.

[0033] Figure 7 Schematic diagram for calculating the carbonization degree of active carbon fixation cold bonding coarse bone.

[0034] Figure 8 The graph is a result of the carbonization degree of the coarse bone actively fixed with carbon and cold bonded in Comparative Example 1, Comparative Example 2 and Example 1.

[0035] Fig. 9 The single particle compressive strength results of actively carbonized cold-bonded coarse aggregate with different oxygen curing ages and actively carbonized cold-bonded coarse aggregate after carbonization. DETAILED DESCRIPTION

[0036] The present invention provides an active carbon fixation cold bonding coarse aggregate and a preparation method and application thereof. To make the purpose, technical scheme and effect of the present invention clearer and more specific, the present invention is further described in detail below. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0037] Unless otherwise defined, all technical terms and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.

[0038] The embodiment of the present invention provides a method for preparing active carbon-fixing cold-bonding coarse aggregate, wherein: Figure 1 and Figure 2 As shown, the following steps are included:

[0039] S1. Mix 90 parts of construction waste slurry powder, 10 parts of cement, and 0-15 parts of alkali-modified biochar by weight to obtain a mixture; wherein the construction waste slurry powder is obtained by hardening the construction waste slurry and then ball milling; the alkali-modified biochar is obtained by soaking the biochar in an alkali metal hydroxide solution and then drying; wherein the alkali-modified biochar does not take 0 parts;

[0040] S2. The mixture is subjected to cold bonding granulation and curing to obtain the active carbon-fixing cold bonding coarse aggregate.

[0041] The present invention uses relatively cheap construction waste slurry powder as a filler and the main carrier of carbon fixation, biochar as a carbon absorption material (so that carbon dioxide in the air can continuously enter the interior of the aggregate and react with the construction waste slurry powder), and cement as a binder, and the raw material cost is relatively low; further, cold bonding granulation is used to effectively gather the raw materials to prepare active carbon fixation cold bonding coarse aggregate. Compared with other granulation technologies, cold bonding granulation can reduce energy consumption, reduce carbon dioxide generated in the production process, protect the environment, and save natural resources. At the same time, it can ensure that the prepared coarse aggregate has a large porosity, ensuring that CO2 can effectively enter the interior of the aggregate, so that the construction waste slurry therein captures and seals CO2. The active carbon fixation cold bonding coarse aggregate prepared by the present invention can achieve the capture and sealing of CO2, and each 1kg of active carbon fixation cold bonding coarse aggregate can absorb 100 to 180g of CO2. The mechanical properties of the active carbon fixation cold bonding coarse aggregate are significantly improved after carbonization (CO2 is converted into solid calcium carbonate by reacting with construction waste slurry powder and alkali-modified biochar, thereby improving the compressive strength of the aggregate). The single particle crushing strength will increase by 8% to 75%, maintaining between 2.5 and 5.5 MPa; the water absorption rate will remain between 11% and 14%; the apparent density will increase by 4% to 10%, maintaining at 1550 g / cm 3 ~1800g / cm 3 Between. Construction waste slurry will cause pollution to the land when it is landfilled. The present invention uses construction waste slurry powder as raw material, realizes the resource utilization of construction waste slurry, reduces the problems caused by treatment and landfill, and is also beneficial to the sustainable development of building materials. The shortage of natural stone and the energy consumption and environmental pollution that may be caused by mountain blasting during the mining of coarse aggregates, and the active carbon fixation cold bonding coarse aggregate provided by the present invention can be used instead of natural aggregate, reducing the damage to the environment caused by the mining of natural aggregates. The sale of the active carbon fixation cold bonding coarse aggregate can also bring economic benefits. In addition, due to the large demand for concrete, the demand for aggregates is also large, so the present invention can significantly increase the recycling of construction waste slurry.

[0042] The active carbon fixation cold bonding coarse aggregate provided by the present invention can absorb CO2 gas in the atmosphere and can also be used as a coarse aggregate component in concrete, and has the advantages of energy saving, environmental protection, and stable working performance of concrete when used as concrete coarse aggregate.

[0043] The construction waste slurry powder contains a large amount of components that can react with CO2 to form stable CaCO3 (mainly calcium hydroxide (CH), calcium silicate hydrate (CSH) gel, ettringite (Aft) and monosulfide hydrated calcium sulfoaluminate (Afm), etc.), which can absorb and fix CO2 in large quantities. The construction waste slurry is crushed and ground into aggregate, which greatly increases the specific surface area.

[0044] Cement is also a carbon-absorbing material with great potential. It contains a large amount of calcium-containing substances, which can react with CO2 in the air to form calcium carbonate, thereby realizing the storage of CO2. However, due to the compactness of the cement matrix and the formation of a dense calcium carbonate layer after carbonization, the development of carbonization is hindered. It can be observed in concrete structures that have been in service for a long time that the carbonization development is often only on the surface. In order to fully improve the carbon fixation capacity of coarse aggregate, the present invention adds alkali-modified biochar to increase the degree of carbonization. Alkali-modified biochar has a rich pore structure, which can effectively increase the number of connected pores inside the coarse aggregate, and can ensure that there are sufficient CO2 circulation channels inside the coarse aggregate, thereby improving the carbon fixation capacity of the coarse aggregate. And because alkali-modified biochar is inert to react and does not react with the matrix, its pore structure is stable and does not change over time. Furthermore, the alkali-modified biochar has alkaline sites, mainly alkaline functional groups (when it is a biomass raw material, the inorganic salts contained therein remain in the structure of the biochar during the heating process due to their high stability, showing alkaline functional groups). Since CO2 molecules are acidic substances, alkaline functional groups are more attractive to them. In addition, during cement hydration, the alkali-modified biochar has a huge specific surface area and can act as a nodule site during cement hydration, greatly promoting the degree of cement hydration. In addition, although the addition of alkali-modified biochar can increase the degree of carbonization, at the same time, due to its special pore structure, its strength is relatively low, and it will become a weak point at a large dosage, thereby reducing the strength of the coarse aggregate. Adding too much alkali-modified biochar will introduce too much inert porous material, resulting in a decrease in the performance of the coarse aggregate in all aspects. The use of the above-mentioned mass fraction of alkali-modified biochar can improve the carbon fixation capacity of the coarse aggregate and ensure that the coarse aggregate has sufficient strength.

[0045] The inventors found that a small amount of biochar (unmodified) added to coarse aggregate can enhance the hydration degree of coarse aggregate due to its internal curing effect, thereby improving the pore structure of coarse aggregate; however, it reduces the efficiency of CO2 molecules diffusing into the interior of coarse aggregate, resulting in a decrease in carbon absorption. Therefore, the present invention uses an alkali metal hydroxide solution to soak and clean biochar, which can improve the pore structure of biochar. This is mainly because the alkali metal hydroxide solution can react with substances accumulated in the pores of biochar, so that the substances accumulated in the pores of biochar are dissolved in the solution and then discharged, releasing the pore structure; and the alkali metal hydroxide solution does not change the other properties of the biochar itself. In addition, the number of alkaline functional groups in the alkali-modified biochar obtained after soaking in an alkali metal hydroxide solution will be increased to a certain extent, and the adsorption capacity for CO2 will also be improved. In addition, the alkali-modified biochar is rich in Na + or K + , and Na + or K + It will enter the interlayer of CSH gel, increase the rigidity of gel structure, and thus improve the strength of coarse aggregate. + and K + The CSH gel structure will be dissociated, resulting in negative effects. The use of the alkali-modified biochar in the mass fraction described in the embodiment of the present invention can ensure the strength and carbon fixation capacity of the coarse aggregate without causing the gel structure to dissociate.

[0046] The actively carbonized cold-bonded coarse aggregate provided by the embodiment of the present invention can absorb carbon in a high concentration CO2 environment (10%±1%), with a complete carbonization time of 24 to 72 hours, and can also absorb carbon in a low concentration CO2 environment (natural environment, 0.04%), with a complete carbonization time of 7 to 56 days.

[0047] In step S1, 90 parts of construction waste slurry powder, 10 parts of cement, and 0-15 parts of alkali-modified biochar are mixed. For example, 90 parts of construction waste slurry powder, 10 parts of cement, and 1 part of alkali-modified biochar are mixed; 90 parts of construction waste slurry powder, 10 parts of cement, and 5 parts of alkali-modified biochar are mixed; 90 parts of construction waste slurry powder, 10 parts of cement, and 10 parts of alkali-modified biochar are mixed; or, 90 parts of construction waste slurry powder, 10 parts of cement, and 15 parts of alkali-modified biochar are mixed.

[0048] In some embodiments, the cement is ordinary Portland cement.

[0049] In some embodiments, the method for preparing alkali-modified biochar specifically comprises the following steps:

[0050] Step A, adding biochar powder to deionized water, stirring, standing, discarding the supernatant, and obtaining a precipitate;

[0051] Step B, adding an alkali metal hydroxide solution to the precipitate, stirring, allowing to stand, and discarding the supernatant to obtain a precipitate;

[0052] Step C, adding deionized water to the precipitate, stirring, standing, and discarding the supernatant to obtain a precipitate;

[0053] Step D, repeating step C several times, drying the obtained precipitate to obtain the alkali-modified biochar.

[0054] In some embodiments, the alkali metal hydroxide solution includes at least one of a potassium hydroxide solution and a sodium hydroxide solution, but is not limited thereto.

[0055] In some embodiments, the concentration of the alkali metal hydroxide solution is 1 mol / L, which is the optimal concentration for improving the performance of biochar. A higher concentration will destroy the internal microstructure of the biochar and cause performance degradation, while a lower concentration will result in insignificant performance improvement.

[0056] In some embodiments, the particle size of the biochar powder is less than 150 μm; the particle size of the construction waste slurry powder is less than 150 μm.

[0057] In step S2, in some embodiments, the step of cold bonding and granulating the mixture specifically includes:

[0058] The mixed materials are fed into a disc granulator in batches for cold bonding granulation, and water is sprayed during the feeding process, with the total water consumption being 15% to 20% of the mass of the mixed materials.

[0059] The mixture is fed into a disc granulator, and water is evenly sprayed during the feeding process and the disc is rotated continuously. Under the action of water and the centrifugal force of the rotating disc, the mixture begins to gradually bond together, and through continuous rolling, the particle size of the particles gradually increases, and a cold-bonded coarse aggregate embryo is obtained. In addition, too much or too little water will affect the forming of the aggregate, resulting in low granulation efficiency or failure to obtain suitable aggregate. For example, the total water consumption is 15%, 16%, 17%, 18%, 19% or 20% of the mass of the mixture. Specifically, water is sprayed through a liquid distributor so that the water can be evenly sprayed on the mixture. In this embodiment, the time of the cold bonding granulation can be set according to actual needs. For example, it can be 5 to 10 minutes.

[0060] In some embodiments, the parameters of the disc granulator are: the disc inclination angle is 45-60° (for example, it can be 45°, 48°, 50°, 52°, 55°, 58° or 60°, etc.), the disc diameter is 0.5-2m (for example, it can be 0.5m, 0.8m, 1m, 1.2m, 1.5m, 1.8m or 2m, etc.), the edge height is 15-20cm (for example, it can be 15cm, 16cm, 17cm, 18cm, 19cm or 20cm, etc.), and the rotation speed is 15-35rpm (for example, it can be 15rpm, 20rpm, 25rpm, 30rpm or 35rpm, etc.).

[0061] In some embodiments, the particle size of the active carbon fixation cold bonding coarse aggregate is greater than 4.75 mm, specifically, it can be 4.75 to 16 mm. The mixture is cold bonded and granulated to obtain a cold bonded coarse aggregate embryo, the aggregate embryo is passed through a sieve with an aperture of 4.75 mm and 16 mm, and a cold bonded coarse aggregate embryo with a particle size of 4.75 to 16 mm is selected and placed in a ventilated place for 24 hours, and then cured to obtain an active carbon fixation cold bonding coarse aggregate with a particle size of 4.75 to 16 mm.

[0062] In some embodiments, the curing conditions are: sealed water bath curing at a temperature of 20±2° C. for at least 28 days. The water bath can ensure that the aggregate has sufficient moisture, so that the hydration of the binder (cement) can continue.

[0063] In some embodiments, the curing conditions are: constant temperature and humidity curing, the temperature is 20±2° C., the humidity is greater than 95%, and the time is at least 28 days.

[0064] An embodiment of the present invention further provides an active carbon-fixing cold-bonding coarse aggregate, wherein the active carbon-fixing cold-bonding coarse aggregate is prepared by the preparation method of the present invention as described above.

[0065] A third aspect of the present invention provides a carbon fixation method, wherein the actively carbon-fixing cold-bonded coarse aggregate as described above in the embodiment of the present invention is placed in an environment to be carbon-fixed, and the actively carbon-fixing cold-bonded coarse aggregate is used to absorb carbon dioxide to perform carbon fixation.

[0066] The present invention will be further described below by means of specific examples.

[0067] The ordinary Portland cement used in the following examples is Conch brand commercial product P·O 42.5 ordinary Portland cement, which complies with GB 175-2007); the biochar used in the following examples is produced by Henan Zhongxin Blue Sky Environmental Protection Equipment Co., Ltd., which is obtained by pyrolysis of bamboo as raw material under a nitrogen environment. The heating rate during the pyrolysis process is 10°C / min and the pyrolysis temperature is 500°C.

[0068] The chemical compositions of the raw materials in the following examples and comparative example 1 are shown in Table 1.

[0069] Table 1. Chemical composition of raw materials

[0070]

[0071] Example 1

[0072] This embodiment provides a method for preparing active carbon-fixing cold-bonding coarse aggregate, comprising the following steps:

[0073] (1) Provide construction waste slurry powder

[0074] The construction waste slurry (unused concrete slurry in the mixer truck transported out of the mixing station) is hardened and crushed, and then dried, ball-milled and screened to obtain construction waste slurry powder with a particle size of less than 150μm; its physical picture and SEM are shown in the following figure Figure 2 shown.

[0075] (2) Providing biochar powder

[0076] The biochar was ground and screened to obtain biochar powder with a particle size of less than 150 μm; its physical picture and SEM are shown in the following figure. Figure 3 shown.

[0077] (3) Preparation of alkali-modified biochar

[0078] Step A: add biochar powder to deionized water at a mass ratio of 1:10, stir with a stirrer for 24 hours at a speed of 550±10rpm, let stand for 24 hours, pour out the upper clear liquid after the liquid is separated, and obtain a precipitate.

[0079] Step B, adding 1 mol / L NaOH solution (the mass ratio of the biochar powder in step A to the NaOH solution is 1:10) to the precipitate and stirring for 24 hours at a speed of 550±10 rpm. After standing for 24 hours, pouring out the upper clear liquid after the liquid is separated to obtain a precipitate;

[0080] Step C, pouring deionized water into the precipitate (the mass ratio of the biochar powder in step A to the deionized water is 1:10), stirring for 15 minutes, standing for 24 hours, and pouring out the supernatant after the liquid is separated to obtain a precipitate;

[0081] Step D: After repeating step C four times (ie, performing step C five times in total), the obtained precipitate is dried in a drying oven at 65° C. until the mass no longer changes, thereby obtaining alkali-modified biochar.

[0082] (4) Preparation of active carbon fixation cold bonding coarse aggregate

[0083] like Figure 4 As shown, by weight, 90 parts of construction waste slurry powder, 10 parts of ordinary Portland cement, and 5 parts of alkali-modified biochar were added into a mixer, and stirred for 10 minutes to obtain a mixture.

[0084] The mixture is put into a disc granulator for granulation, and water is evenly sprayed during the feeding process (the total water consumption is 20% of the mass of the raw materials) and the disc granulator is rotated continuously. When the aggregate reaches the expected size, the dry powder of the mixture is sprinkled into the granulator in the final stage, so that the outer surface of the aggregate is in a dry state, and after screening with a 4.75 mm sieve, a cold-bonded coarse aggregate embryo with a particle size greater than 4.75 mm is obtained (the cold-bonded coarse aggregate embryo with a particle size less than 4.75 mm is continuously returned to the disc granulator for granulation), wherein the parameters of the disc granulator are: the disc inclination angle is 45°, the disc diameter is 1 m, the edge height is 15 cm, and the rotation speed is 20 rpm;

[0085] The cold-bonded coarse aggregate embryo is water-bath cured at a temperature of 20±2°C for 28 days (specifically, it is placed in a sealed bag and injected with water at 20±2°C, and finally the bag mouth is sealed), then taken out and wiped dry, and then placed in a vacuum drying oven, the drying temperature is controlled to be 45°C, and dried until the quality no longer changes, to obtain an actively carbon-fixing cold-bonded coarse aggregate (which can replace natural aggregate and be added to concrete for use).

[0086] Comparative Example 1

[0087] This comparative example provides a method for preparing active carbon-fixing cold-bonded coarse aggregate, which is different from Example 1 only in that no alkali-modified biochar is added.

[0088] Comparative Example 2

[0089] This comparative example provides a method for preparing active carbon-fixing cold-bonded coarse aggregate, comprising the following steps:

[0090] (1) Provide construction waste slurry powder

[0091] Same as step (1) in Example 1.

[0092] (2) Providing biochar powder

[0093] Same as step (2) in Example 1.

[0094] (3) Preparation of active carbon fixation cold bonding coarse aggregate

[0095] The only difference from step (4) in Example 1 is that the alkali-modified biochar is replaced by biochar powder (unmodified), that is, biochar powder that has not undergone any modification.

[0096] test:

[0097] (1) The particle size distribution of unmodified (or untreated) biochar powder, alkali-modified biochar, construction waste slurry powder and ordinary Portland cement is shown in the figure. Figure 5 shown.

[0098] (2) Carbon fixation capacity test

[0099] The actively carbonized cold-bonded coarse aggregates in Example 1, Comparative Example 1 and Comparative Example 2 were placed in a high CO2 concentration carbonization box (the initial volume concentration of CO2 was 10±1%, the temperature was 20±5°C, and the humidity was 70±5%) and carbonized for 3 days to obtain the carbonized actively carbonized cold-bonded coarse aggregates.

[0100] Then split the carbonized active carbon-fixed cold-bonded coarse aggregate, spray phenolphthalein alcohol solution on the cross section, and after the color development is completed, the result is as follows: Figure 6 As shown in the figure, the purple area is the uncarbonized area, and the surrounding non-colored area is the area that absorbs CO2. It can be seen that the carbon fixation ability in Example 1 is stronger and the carbonization depth is greater. Figure 7 As shown, Figure 6 The carbonization degree of the three actively carbonized cold-bonded coarse aggregates in the calculation is: carbonization degree = S1 / (S1+S2), where S1 is the carbonized area and S2 is the uncarbonized area. The results are as follows: Figure 8 The carbonization degree of the actively carbonized cold-bonded coarse aggregate in Example 1 is 0.43, i.e. 43%, while the carbonization degree of the actively carbonized cold-bonded coarse aggregate in Comparative Example 1 is 0.1, i.e. 10%, and the carbonization degree of the actively carbonized cold-bonded coarse aggregate in Comparative Example 2 is 0.35, i.e. 35%. It can be seen that the addition of alkali-modified biochar can improve the carbon fixation capacity of the actively carbonized cold-bonded coarse aggregate.

[0101] (3) Single particle compressive strength test

[0102] a. Test the single-particle compressive strength of the actively carbonized cold-bonded coarse aggregate with a curing age of 3 days and the single-particle compressive strength of the actively carbonized cold-bonded coarse aggregate with a curing age of 3 days after carbonization:

[0103] Take the cold-bonded coarse aggregate embryos in Example 1, Comparative Example 1 and Comparative Example 2, respectively, and water-bath cure them at a temperature of 20±2° C. for 3 days, take them out from the water-bath and wipe them dry, then put them into a vacuum drying oven, control the drying temperature to 45° C., and dry them until the quality no longer changes to obtain active carbon-fixing cold-bonded coarse aggregates, and perform a single-particle compressive strength test on a portion of the active carbon-fixing cold-bonded coarse aggregates in each example;

[0104] Then, another part of the actively carbonized cold-bonded coarse aggregate in each example was placed in a high CO2 concentration carbonization box (the initial volume concentration of CO2 was 10±1%, the temperature was 20±5°C, and the humidity was 70±5%) and carbonized for 3 days to obtain the carbonized actively carbonized cold-bonded coarse aggregate, and a single particle compressive strength test was carried out.

[0105] b. Test the single-particle compressive strength of the actively carbonized cold-bonded coarse aggregate with a curing age of 7 days and the single-particle compressive strength of the actively carbonized cold-bonded coarse aggregate with a curing age of 7 days after carbonization:

[0106] The specific steps are different from step a only in that "curing in a water bath at a temperature of 20±2°C for 3 days" is replaced by "curing in a water bath at a temperature of 20±2°C for 7 days".

[0107] c. Test the single-particle compressive strength of the actively carbonized cold-bonded coarse aggregate with a curing age of 14 days and the single-particle compressive strength of the actively carbonized cold-bonded coarse aggregate with a curing age of 14 days after carbonization:

[0108] The specific steps are different from step a only in that "curing in a water bath at a temperature of 20±2°C for 3 days" is replaced by "curing in a water bath at a temperature of 20±2°C for 14 days".

[0109] d. Test the single-particle compressive strength of the actively carbonized cold-bonded coarse aggregate with a curing age of 28 days and the single-particle compressive strength of the actively carbonized cold-bonded coarse aggregate with a curing age of 28 days after carbonization:

[0110] The specific steps are different from step a only in that "curing in a water bath at a temperature of 20±2°C for 3 days" is replaced by "curing in a water bath at a temperature of 20±2°C for 28 days".

[0111] The results are as follows Fig. 9 As shown. By adding alkali-modified biochar, it is possible to ensure that the active carbon fixation cold bonding coarse aggregate has sufficient strength, and after carbonization, the strength of the active carbon fixation cold bonding coarse aggregate is significantly improved.

[0112] In summary, the present invention provides an active carbon fixation cold bonding coarse aggregate and its preparation method and application, using relatively low-priced construction waste slurry powder as filler and main carrier for carbon fixation, biochar as carbon absorption material, cement as binder, and low raw material cost; further using cold bonding granulation to effectively gather the raw materials to prepare the active carbon fixation cold bonding coarse aggregate, compared with other granulation technologies, cold bonding granulation can reduce energy consumption, reduce carbon dioxide generated in the production process, protect the environment, save natural resources, and at the same time ensure that the prepared coarse aggregate has a large porosity, ensuring that CO2 can effectively enter the interior of the aggregate, so that the construction waste slurry therein captures and seals CO2. The active carbon fixation cold bonding coarse aggregate prepared by the present invention can absorb 100 to 180 g of CO2 in situ per 1 kg of active carbon fixation cold bonding coarse aggregate. The mechanical properties of the active carbon fixation cold bonding coarse aggregate are significantly improved after carbonization. The crushing strength of a single particle will increase by 8% to 75% and remain between 2.5 and 5.5 MPa; the water absorption rate will remain between 11% and 14%; the apparent density will increase by 4% to 10% and remain at 1550 g / cm 3 ~1800g / cm 3 Between. Construction waste slurry will cause pollution to the land when it is landfilled. The present invention uses construction waste slurry powder as raw material, realizes the resource utilization of construction waste slurry, reduces the problems caused by treatment and landfill, and is also beneficial to the sustainable development of building materials. The shortage of natural stone and the energy consumption and environmental pollution that may be caused by mountain blasting during the mining of coarse aggregates, and the active carbon fixation cold bonding coarse aggregate provided by the present invention can be used instead of natural aggregate, reducing the damage to the environment caused by the mining of natural aggregates. The sale of the active carbon fixation cold bonding coarse aggregate can also bring economic benefits. In addition, due to the large demand for concrete, the demand for aggregates is also large, so the present invention can significantly increase the recycling of construction waste slurry.

[0113] It should be understood that the application of the present invention is not limited to the above examples. For ordinary technicians in this field, improvements or changes can be made based on the above description. All these improvements and changes should fall within the scope of protection of the claims attached to the present invention.

Claims

1. A method for preparing active carbon-fixing cold-bonding coarse aggregate, characterized in that: The steps include: By weight, 90 parts of construction waste slurry powder, 10 parts of cement, and 0-15 parts of alkali-modified biochar are mixed to obtain a mixture; wherein the alkali-modified biochar is not taken as 0 part; The mixture is subjected to cold bonding granulation and curing to obtain the active carbon-fixing cold bonding coarse aggregate; The construction waste slurry powder is obtained by hardening the construction waste slurry and then ball milling it; The alkali-modified biochar is obtained by soaking the biochar in an alkali metal hydroxide solution and then drying it.

2. The preparation method according to claim 1, characterized in that: The particle size of the active carbon-fixing cold-bonding coarse aggregate is greater than 4.75 mm.

3. The preparation method according to claim 1, characterized in that: The cement is ordinary Portland cement.

4. The preparation method according to claim 1, characterized in that: The preparation method of the alkali-modified biochar specifically comprises the following steps: Step A, adding biochar powder to deionized water, stirring, standing, discarding the supernatant, and obtaining a precipitate; Step B, adding an alkali metal hydroxide solution to the precipitate, stirring, allowing to stand, and discarding the supernatant to obtain a precipitate; Step C, adding deionized water to the precipitate, stirring, standing, and discarding the supernatant to obtain a precipitate; Step D, repeating step C several times, drying the obtained precipitate to obtain the alkali-modified biochar.

5. The preparation method according to claim 4, characterized in that: The particle size of the biochar powder is less than 150 μm; the particle size of the construction waste slurry powder is less than 150 μm; The alkali metal hydroxide solution includes at least one of a potassium hydroxide solution and a sodium hydroxide solution.

6. The preparation method according to claim 1, characterized in that: The step of cold bonding and granulating the mixed material specifically comprises: The mixed materials are fed into a disc granulator in batches for cold bonding granulation, and water is sprayed during the feeding process, with the total water consumption being 15% to 20% of the mass of the mixed materials.

7. The preparation method according to claim 6, characterized in that: The parameters of the disc granulator are as follows: the disc inclination angle is 45-60°, the disc diameter is 0.5-2m, the edge height is 15-20cm, and the rotation speed is 15-35rpm.

8. The preparation method according to claim 1, characterized in that: The curing conditions are: sealed water bath curing at a temperature of 20±2°C for at least 28 days; or, the curing conditions are: constant temperature and humidity curing at a temperature of 20±2°C, a humidity greater than 95%, for at least 28 days.

9. An active carbon fixation cold bonding coarse aggregate, characterized in that: The active carbon fixation cold bonding coarse aggregate is prepared by the preparation method described in any one of claims 1 to 8.