Self-compacting basalt fiber ultra-high performance concrete and preparation method thereof
By using specific raw material proportions and mixing processes, the problem of difficult dispersion of basalt fiber concrete has been solved, resulting in high fluidity and ultra-high strength concrete suitable for complex environments, with good economic and social benefits.
Patent Information
- Application Number
- CN202411112127.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-12
AI Technical Summary
Existing basalt fiber reinforced concrete is prone to clumping during the incorporation process, which leads to a decrease in fluidity and mechanical properties. Furthermore, it is difficult to disperse, and existing solutions are complex and costly, limiting its application in practical engineering.
By using a specific raw material ratio and mixing process, quartz sand is first mixed with cement, then mixed with basalt fiber, silica fume, and water-reducing agent, and finally water is added. Through the friction between quartz sand and fiber and the protection of powder, the fiber is evenly dispersed, thereby improving the workability of concrete.
It achieves uniform dispersion of basalt fibers, improves the fluidity and mechanical properties of concrete, with compressive strength exceeding 120MPa and splitting tensile strength exceeding 10MPa, making it suitable for complex environments and offering good economic and social benefits.
Smart Images

Figure BDA0004992538060000081 
Figure BDA0004992538060000082 
Figure BDA0004992538060000091
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of concrete, and specifically relates to a self-compacting basalt fiber ultra-high performance concrete and a preparation method thereof. Background Art
[0002] With the development of economy and technology, the construction industry has gradually increased its requirements for the performance of concrete used. Adding fibers to the concrete matrix can greatly improve the mechanical properties of concrete. The fibers are randomly distributed in the concrete to form a three-dimensional grid, which can play a good connecting role and inhibit the generation of micro cracks in the concrete when it is loaded.
[0003] At present, common fibers added to concrete include steel fibers and carbon fibers, but carbon fibers are expensive and have poor economic benefits when used in concrete. Steel fibers are the most widely used fibers in concrete, but they are easily corroded by harsh environments such as marine environments. Therefore, it may be a reasonable prospect to add cheap, durable, and high-tensile-strength basalt fibers to concrete to form composite materials. However, the aspect ratio of basalt fibers is relatively large (about 270 to 350), which is more than 10 times that of steel fibers. If basalt fibers are added to the concrete matrix, agglomeration is likely to occur, which greatly reduces the fluidity of the concrete paste and the mechanical properties of the concrete after molding. The current solutions are mostly to use chemical agents (such as coupling agents such as KH550 and KH560, graphene oxide dispersion) to modify the surface of basalt fibers or use ultrasonic oscillation dispersion. These methods are not only complicated and costly, but also greatly prolong the preparation cycle of basalt fiber concrete, limiting the development and application of basalt fiber concrete in actual engineering.
[0004] The difficulty in preparing basalt fiber high-performance concrete lies in the dispersion of the fibers. As the amount of fiber added increases, the dispersion becomes increasingly difficult. Increasing the amount of fiber added will not only fail to improve the performance of the concrete, but may even reduce the strength of the concrete. In order to reduce the negative impact of basalt fiber, current basalt fiber concrete usually only incorporates a small amount of basalt fiber. The literature "Orthogonal Experimental Study on Mechanical Properties of Basalt Fiber High-Performance Concrete" (Chen Feng, Chen Xin. Orthogonal Experimental Study on Mechanical Properties of Basalt Fiber High-Performance Concrete [J]. Journal of Civil Engineering and Management, 2013, 030(002): 6-10.) discloses that basalt fiber high-performance concrete has a basalt fiber content of 1.2 kg / m 3 The working performance is optimal when adding a small amount of basalt fiber, but the reinforcing effect on concrete is not obvious, and the compressive strength of basalt fiber high-performance concrete can only reach about 60MPa. Summary of the invention
[0005] In view of this, the object of the present invention is to provide a self-compacting basalt fiber ultra-high performance concrete and a preparation method thereof. The basalt fiber ultra-high performance concrete of the present invention has a compressive strength exceeding 120MPa and a splitting tensile strength exceeding 10MPa, and has ultra-high mechanical properties.
[0006] The present invention provides a self-compacting basalt fiber ultra-high performance concrete, comprising the following raw materials in parts by weight: 75-85 parts of cement, 20-25 parts of silica fume, 80-95 parts of quartz sand, 1-2 parts of water reducer, 18-22 parts of water and 3-5 parts of basalt fiber;
[0007] The method for preparing the self-compacting basalt fiber ultra-high performance concrete comprises the following steps:
[0008] After the quartz sand is mixed with cement for a first stirring, it is mixed with basalt fiber for a second stirring, and then mixed with silica fume and a water reducing agent for a third stirring, and then mixed with water for a fourth stirring to obtain a self-compacting basalt fiber ultra-high performance concrete.
[0009] Preferably, the quartz sand includes first quartz sand, second quartz sand and third quartz sand, the particle size of the first quartz sand is less than 0.425 mm and greater than or equal to 0.25 mm, the particle size of the second quartz sand is less than 0.25 mm and greater than or equal to 0.125 mm, and the particle size of the third quartz sand is less than 0.125 mm and greater than or equal to 0.045 mm;
[0010] Preferably, the weight ratio of the first quartz sand, the second quartz sand and the third quartz sand is 29-35:18-25:30-38.
[0011] Preferably, the basalt fiber is a chopped basalt fiber, the diameter of the chopped basalt fiber is 17-18 μm, the length is 5-6 mm, and the density is 2.6-2.65 g / cm 3 .
[0012] Preferably, the basalt fiber comprises 3.6 to 4.14 parts.
[0013] Preferably, the water reducing agent has a water reducing rate of 24% to 26%.
[0014] Preferably, the preparation raw materials include the following parts by weight: 80 parts of cement, 20 parts of silica fume, 80 parts of quartz sand, 1 part of water reducing agent, 20 parts of water, and 4.14 parts of basalt fiber.
[0015] Preferably, the preparation raw materials include the following parts by weight: 75 parts of cement, 22.5 parts of silica fume, 95 parts of quartz sand, 2 parts of water reducing agent, 19 parts of water, and 3.6 parts of basalt fiber.
[0016] The present invention also provides a method for preparing the self-compacting basalt fiber ultra-high performance concrete described in the above technical solution, comprising the following steps:
[0017] After the quartz sand is mixed with cement for a first stirring, it is mixed with basalt fiber for a second stirring, and then mixed with silica fume and a water reducing agent for a third stirring, and then mixed with water for a fourth stirring to obtain a self-compacting basalt fiber ultra-high performance concrete.
[0018] Preferably, the first stirring time is 30 to 50 seconds, the second stirring time is 2 to 3 minutes, the third stirring time is 1 to 2 minutes, and the fourth stirring time is 10 to 12 minutes.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] The invention provides a self-compacting basalt fiber ultra-high performance concrete, comprising the following raw materials in parts by weight: 75-85 parts of cement, 20-25 parts of silica fume, 80-95 parts of quartz sand, 1-2 parts of water reducer, 18-22 parts of water and 3-5 parts of basalt fiber; a method for preparing the self-compacting basalt fiber ultra-high performance concrete comprises the following steps: mixing quartz sand with cement for a first stirring, then mixing with basalt fiber for a second stirring, then mixing with silica fume and water reducer for a third stirring, and then mixing with water for a fourth stirring to obtain the self-compacting basalt fiber ultra-high performance concrete.
[0021] The present invention utilizes the friction between quartz sand and fiber to fully disperse the fiber. The present invention first mixes and stirs the aggregate quartz sand with the powder cement. The cement particles can appropriately wrap the quartz sand particles. After the basalt fiber is subsequently added, the excessive friction of the quartz sand on the fiber can be reduced, and the basalt fiber is protected from being damaged by the quartz sand (that is, the protection of the powder prevents the basalt fiber from being damaged by excessive friction of the quartz sand). After the basalt fiber is evenly dispersed, water is added to mix, which prevents the problem of uneven fiber dispersion caused by the wet powder (cement, silica fume) after the water is added, and the wet powder wraps the undispersed basalt fiber. Therefore, the amount of basalt fiber can be appropriately increased, and the mechanical properties of basalt fiber ultra-high performance concrete can be improved. The present invention greatly reduces the complexity of basalt fiber dispersion, which is conducive to the application of basalt fiber in practical engineering. The present invention optimizes the mix ratio and improves the fiber dispersion, thereby making the concrete obtain ultra-high strength and greatly improving the working performance of the concrete paste after the basalt fiber is added. It not only solves the common fiber economy problem in concrete, but also improves the low fluidity problem of the concrete paste caused by the addition of basalt fiber, and has good economic and social benefits.
[0022] The present invention uses basalt fiber and concrete in combination, and utilizes the connecting effect of the fiber to effectively prevent cracking, strengthen and toughen the concrete, thereby improving the performance of the concrete. Compared with steel fiber and carbon fiber, basalt fiber is more economical, environmentally friendly, has excellent durability, and is more suitable for actual engineering and various complex environments. DETAILED DESCRIPTION
[0023] The present invention provides a self-compacting basalt fiber ultra-high performance concrete, comprising the following raw materials in parts by weight: 75-85 parts of cement, 20-25 parts of silica fume, 80-95 parts of quartz sand, 1-2 parts of water reducer, 18-22 parts of water and 3-5 parts of basalt fiber;
[0024] The method for preparing the self-compacting basalt fiber ultra-high performance concrete comprises the following steps:
[0025] After the quartz sand is mixed with cement for a first stirring, it is mixed with basalt fiber for a second stirring, and then mixed with silica fume and a water reducing agent for a third stirring, and then mixed with water for a fourth stirring to obtain a self-compacting basalt fiber ultra-high performance concrete.
[0026] In the present invention, unless otherwise specified, the materials and equipment used are commercially available products in the art.
[0027] In the present invention, the weight percentage of cement in the raw material is preferably 75 to 80. In the present invention, the cement is preferably PO 52.5 ordinary Portland cement.
[0028] Based on the weight of cement, the weight of silica fume in the raw material is preferably 20 to 22.5 parts.
[0029] In the present invention, the silica fume is preferably grade I silica fume.
[0030] Based on the weight of cement, the weight of quartz sand in the raw material is preferably 85 to 90 parts.
[0031] In the present invention, the quartz sand preferably includes first quartz sand, second quartz sand and third quartz sand, the particle size of the first quartz sand is less than 0.425 mm (40 mesh) and greater than or equal to 0.25 mm (60 mesh), the particle size of the second quartz sand is less than 0.25 mm and greater than or equal to 0.125 mm (120 mesh), and the particle size of the third quartz sand is less than 0.125 mm and greater than or equal to 0.045 mm (325 mesh); the weight ratio of the first quartz sand, the second quartz sand and the third quartz sand is preferably 29-35:18-25:30-38, and more preferably 29.3:19.5:31.2 or 34.8:23.1:37.1.
[0032] Based on the weight of cement, the weight of the water reducing agent in the raw material is preferably 1 part.
[0033] In the present invention, the water reducing rate of the water reducing agent is preferably 24% to 26%, more preferably 25%, and the water reducing agent is preferably a polycarboxylic acid high performance water reducing agent powder.
[0034] Based on the weight of cement, the weight of water in the raw material is preferably 19 to 20 parts.
[0035] Based on the weight of cement, the weight of basalt fiber in the raw material is preferably 3.6 to 4.14 parts. The present invention adds a large amount of basalt fiber to the concrete without uneven dispersion, so that the concrete has a greater strength improvement and achieves excellent working performance.
[0036] In the present invention, the basalt fiber is preferably chopped basalt fiber, the diameter of the chopped basalt fiber is preferably 17-18 μm, the length is preferably 5-6 mm, and the density is preferably 2.6-2.65 g / cm 3 ; The aspect ratio is 270 to 350. The surface of the chopped basalt fiber is preferably coated with a silane impregnant, and the preparation method of the chopped basalt fiber is preferably: after melting and drawing the basalt, soak it in the silane impregnant, take it out after soaking, dry it, and then cut it to obtain the chopped basalt fiber. The function of the silane impregnant is to reduce the phenomenon of loose and broken fibers during fiber production. The elastic modulus of the basalt fiber is preferably 76GPa to 76.2GPa, more preferably 76.1GPa, the tensile strength is preferably 1500 to 1600MPa, and the ultimate elongation is preferably 3.01%. By adding basalt fibers to the present invention, there is less fiber agglomeration in the concrete, and the obtained concrete has good mechanical properties and fluidity.
[0037] In the present invention, the self-compacting basalt fiber ultra-high performance concrete preferably includes the following raw materials in parts by weight: 80 parts of cement, 20 parts of silica fume, 80 parts of quartz sand, 1 part of water reducer, 20 parts of water, and 4.14 parts of basalt fiber;
[0038] Or 75 parts of cement, 22.5 parts of silica fume, 95 parts of quartz sand, 2 parts of water reducer, 19 parts of water, and 3.6 parts of basalt fiber. The raw material ratio of the present invention can obtain concrete with good mechanical properties.
[0039] The present invention also provides a method for preparing the self-compacting basalt fiber ultra-high performance concrete described in the above technical solution, comprising the following steps:
[0040] After the quartz sand is mixed with cement for a first stirring, it is mixed with basalt fiber for a second stirring, and then mixed with silica fume and a water reducing agent for a third stirring, and then mixed with water for a fourth stirring to obtain a self-compacting basalt fiber ultra-high performance concrete.
[0041] In the present invention, the stirring rate of the first stirring is preferably 50 r / min, and the time is preferably 30 to 50 s.
[0042] In the present invention, the stirring rate of the second stirring is preferably 50 r / min, and the time is preferably 2 to 3 min.
[0043] In the present invention, the stirring rate of the third stirring is preferably 50 r / min, and the time is preferably 1 to 2 min.
[0044] In the present invention, the stirring rate of the fourth stirring is preferably 50 r / min, and the time is preferably 10 to 12 min.
[0045] The present invention disperses the fibers through the friction between the aggregate and the basalt fibers. The specific concrete preparation and mixing process of the present invention effectively improves the working performance of the concrete, enables the expansion of the concrete to exceed 600 mm, and achieves the self-compacting characteristics of flowing by its own gravity without vibration and completely filling the formwork.
[0046] The present invention adopts a specific raw material mix ratio, mixing method and quartz sand grading to enable basalt fiber ultra-high performance concrete to maintain ultra-high mechanical properties on the basis of self-compacting characteristics. The present invention solves the problem of difficult dispersion of basalt fiber and complicated dispersion steps, improves the fluidity of concrete, and paves the way for the application of basalt fiber concrete in practical engineering.
[0047] In order to further illustrate the present invention, the self-compacting basalt fiber ultra-high performance concrete and the preparation method thereof provided by the present invention are described in detail below in combination with embodiments, but they should not be construed as limiting the scope of protection of the present invention.
[0048] In the embodiments and comparative examples of the present invention, the basalt fibers used have a diameter of 18 μm, a length of 6 mm, and a density of 2.65 g / cm 3 The elastic modulus is 76.1GPa, the tensile strength is 1600MPa, and the ultimate elongation is 3.01%; the cement is P.O52.5 ordinary Portland cement; the water reducer is polycarboxylic acid high-performance water reducer powder, and the water reduction rate is 25%.
[0049] Example 1
[0050] The self-compacting basalt fiber ultra-high performance concrete consists of the following raw materials by weight: 80 parts of cement, 20 parts of silica fume, 80 parts of quartz sand, 1 part of water reducer, 20 parts of water, and 4.14 parts of basalt fiber.
[0051] Quartz sand of different mesh sizes is calculated by weight: 40-60 mesh 29.3 parts, 60-120 mesh 19.5 parts, 120-325 mesh 31.2 parts.
[0052] The specific stirring steps of the preparation method are as follows:
[0053] (1) Mix quartz sand of different mesh sizes with cement and stir for 30 seconds;
[0054] (2) slowly adding basalt fiber to the mixture of step (1), and stirring for 2 minutes;
[0055] (3) Mix silica fume and water reducer and add to the mixture of step (2), stirring for 1 min;
[0056] (4) adding water to the mixture of step (3), and continuing stirring for 10 minutes to obtain basalt fiber ultra-high performance concrete.
[0057] Example 2
[0058] The self-compacting basalt fiber ultra-high performance concrete consists of the following raw materials by weight: 75 parts of cement, 22.5 parts of silica fume, 95 parts of quartz sand, 2 parts of water reducer, 19 parts of water, and 3.6 parts of basalt fiber.
[0059] Quartz sand of different mesh sizes is calculated by weight: 40-60 mesh 34.8 parts, 60-120 mesh 23.1 parts, 120-325 mesh 37.1 parts.
[0060] The preparation method of the self-compacting basalt fiber ultra-high performance concrete in this embodiment is the same as that in Embodiment 1, and the only difference from Embodiment 1 is the ratio of raw materials.
[0061] Comparative Example 1
[0062] The only difference from Example 1 is the preparation method; the raw material ratio is the same as that of Example 1.
[0063] The specific stirring steps of the preparation method are as follows:
[0064] (1) Mix quartz sand of different mesh sizes with cement and stir for 30 seconds;
[0065] (2) Mix silica fume and water reducer and add to the mixture of step (1), stirring for 1 min;
[0066] (3) adding water to the mixture of step (2) and continuing stirring for 5 min;
[0067] (4) Slowly add basalt fiber to the mixture of step (3) and continue stirring for 7 minutes to obtain basalt fiber concrete.
[0068] Comparative Example 2
[0069] The only difference from Example 1 is the preparation method; the raw material ratio is the same as that of Example 1.
[0070] The specific stirring steps of the preparation method are as follows:
[0071] (1) Mix quartz sand of different mesh sizes with cement and stir for 30 seconds;
[0072] (2) Mix silica fume and water reducer and add to the mixture of step (1), stirring for 1 min;
[0073] (3) Mix water and basalt fiber and add them together to the mixture of step (2), and continue stirring for 12 minutes to obtain basalt fiber concrete.
[0074] Comparative Example 3
[0075] The only difference from Example 1 is that the specification of the quartz sand used is: 60-120 mesh, and the other raw material ratios are the same as those in Example 1.
[0076] The preparation method is the same as that in Example 1, and the only difference from Example 1 is the specifications of the quartz sand.
[0077] Comparative Example 4
[0078] The basalt fiber ultra-high performance concrete consists of the following raw materials by mass: 90 parts of cement, 13.5 parts of silica fume, 83 parts of quartz sand, 3.1 parts of water reducer, 14.5 parts of water, and 5.5 parts of basalt fiber.
[0079] The preparation method and the quartz sand mesh number (ratio) of this comparative example are the same as those of Example 1, and the only difference from Example 1 is the ratio.
[0080] Comparative Example 5
[0081] The basalt fiber ultra-high performance concrete consists of the following raw materials by mass: 80 parts of cement, 12 parts of silica fume, 101.2 parts of quartz sand, 2.3 parts of water reducer, 14.7 parts of water, and 2.27 parts of basalt fiber.
[0082] The preparation method and the quartz sand mesh number (ratio) of this comparative example are the same as those of Example 1, and the only difference from Example 1 is the ratio.
[0083] Comparative Example 6
[0084] The basalt fiber ultra-high performance concrete consists of the following raw materials by mass: 85 parts of cement, 21.25 parts of silica fume, 116.8 parts of quartz sand, 3.18 parts of water reducer, 23.37 parts of water, and 1.31 parts of basalt fiber.
[0085] The preparation method and the quartz sand mesh number (ratio) of this comparative example are the same as those of Example 1, and the only difference from Example 1 is the ratio.
[0086] Test Case
[0087] After Example 1, Comparative Example 1 and Comparative Example 2 were prepared, three 1 kg concrete paste samples were randomly taken and subjected to dispersion tests; and after the preparation of Examples 1 to 2 and Comparative Examples 1 to 6, flowability tests and mold filling were performed.
[0088] The curing conditions of the molded test blocks are: 1 day of natural curing and demoulding, then placed in an 80°C steam curing box for 3 days, and then continued to cure in a standard curing box with a temperature of 22°C and a humidity of 95% for 28 days.
[0089] The basalt fiber dispersion test was carried out according to DL / T 5797-2019 "Construction Specifications for Fiber Concrete in Hydropower and Water Conservancy Projects"; the compressive strength, splitting strength and expansion of the basalt fiber ultra-high performance concrete of each embodiment and each comparative example were tested according to GB / T 50081-2019 "Concrete Physical and Mechanical Properties Test Method Standard". The specific performance tests of Examples 1 to 2 and Comparative Examples 1 to 6 are as follows:
[0090] (1) Basalt fiber dispersion test: After the preparation of Example 1 and Comparative Examples 1-2, three 1 kg concrete slurry samples were randomly taken, and the concrete slurry samples were placed in a container 10 times larger than their own volume. After being rinsed with water, basalt fibers were obtained by filtering with a sieve, which were placed in a container, dried and weighed.
[0091] (2) Fluidity test: Pour the prepared slurry into a standard slump bucket and lift the slump bucket vertically within 3 to 5 seconds. When the slurry stops diffusing or the diffusion time reaches 50 seconds, use a steel ruler to measure the maximum diameter of the slurry twice.
[0092] (3) Compressive strength test: The test blocks of Examples 1 to 2 and Comparative Examples 1 to 4 that had been cured were subjected to a compressive strength test using a universal press at a loading rate of 1.2 MPa / s.
[0093] (4) Splitting tensile strength test: The test blocks of Examples 1 to 2 and Comparative Examples 1 to 4 that have been cured are subjected to a splitting compressive strength test using a universal press at a loading rate of 0.12 MPa / s.
[0094] The test results of basalt fiber dispersion are shown in Table 1; the test results of mechanical properties and fluidity are shown in Table 2.
[0095] Table 1 Basalt fiber dispersion test results
[0096]
[0097] According to the "Construction Specification for Fiber Concrete in Hydropower and Water Conservancy Projects" (DL / T 5797-2019), the actual mass of the measured fiber cannot exceed or be less than 10% of the theoretical mass. Example 1 meets the requirements, while Comparative Examples 1 to 2 do not meet the requirements.
[0098] Common concrete density is 2400kg / m 3 In Example 1 of the present invention, each m 3 The basalt fiber content of basalt fiber concrete is 20.18×2400=48.43(kg), i.e. 48.43kg / m 3 , which is about 40 times the basalt fiber content in the literature "Orthogonal Experimental Study on Mechanical Properties of Basalt Fiber High Performance Concrete" (Chen Feng, Chen Xin. Orthogonal Experimental Study on Mechanical Properties of Basalt Fiber High Performance Concrete [J]. Journal of Civil Engineering and Management, 2013, 030(002): 6-10.), and the present invention achieves uniform dispersion.
[0099] Table 2 Performance test results
[0100]
[0101]
[0102] It can be seen from the fiber dispersion results that by using the preparation method of the present invention, the dispersion of basalt fibers can be significantly improved without using other more complicated steps. The fibers can be fully dispersed by utilizing the friction between quartz sand and fibers. By mixing aggregates and powder materials, powder cement can serve as a buffer between quartz sand and fibers. The protection of the powder material prevents the basalt fibers from being damaged (broken, worn and thinned) due to friction.
[0103] It can be seen from the fluidity test results that the expansion degree of Example 1 is significantly better than that of Comparative Examples 1 to 4. This is because after the quartz sand grading is optimized, during the mixing stage, a part of the slurry formed after the water and the cementitious material are fully mixed is filled in the gaps between the quartz sands, and the other part is adsorbed on the surface of the quartz sand to form a slurry coating layer, resulting in a decrease in the friction between the raw materials; with the increase of the quartz sand particle size and the expansion of the continuously graded quartz sand particle size range, the unit specific surface area of the aggregate decreases, and the slurry coating layer that plays a wetting and lubricating role becomes thicker, resulting in an increase in the expansion degree of the mixture and an improvement in working performance; with the optimization of the preparation process, the basalt fiber is more evenly dispersed in the concrete slurry and the agglomeration phenomenon is improved, thereby improving the slurry fluidity. Too much or too little water-cement ratio and fiber content will reduce the mechanical properties of concrete: 1) When the water-cement ratio is too low, the water required for cement hydration is insufficient and cement hydration is incomplete, which leads to reduced concrete strength; when the water-cement ratio is too high, the free water in the concrete increases. These free waters do not participate in the cement hydration reaction and will gradually evaporate during the concrete hardening process, leaving more pores and voids inside the concrete, which will lead to a decrease in concrete strength; 2) When the fiber content is too low, the fiber's connecting effect is not obvious and the improvement in concrete strength is small; when the fiber content is too high, it is more difficult to disperse the fibers inside the concrete and internal defects will increase, which will also cause a decrease in concrete strength.
[0104] It can be seen from the mechanical properties results that by using the preparation process and mix ratio of the present invention, due to the improvement of fiber dispersion, the internal defects of the concrete matrix are reduced, the reinforcement effect of basalt fiber is improved, the maximum compressive strength exceeds 120MPa, and the maximum splitting tensile strength exceeds 10MPa.
[0105] Example 1 uses the preparation method and ratio optimization of the present invention to achieve an expansion degree of 600 mm, while the compressive strength exceeds 120 MPa and the splitting tensile strength exceeds 10 MPa, and has the multiple advantages of self-compacting and ultra-high performance.
[0106] Although the above-mentioned embodiments have made a detailed description of the present invention, they are only some embodiments of the present invention, rather than all embodiments. People can also obtain other embodiments based on the embodiments of the present invention without creative work, and these embodiments all fall within the scope of protection of the present invention.
Claims
1. A self-compacting basalt fiber ultra-high performance concrete, characterized in that: The preparation material comprises the following raw materials in parts by weight: 75-85 parts of cement, 20-25 parts of silica fume, 80-95 parts of quartz sand, 1-2 parts of water reducing agent, 18-22 parts of water and 3-5 parts of basalt fiber; The method for preparing the self-compacting basalt fiber ultra-high performance concrete comprises the following steps: After the quartz sand is mixed with cement for a first stirring, it is mixed with basalt fiber for a second stirring, and then mixed with silica fume and a water reducing agent for a third stirring, and then mixed with water for a fourth stirring to obtain a self-compacting basalt fiber ultra-high performance concrete.
2. The self-compacting basalt fiber ultra-high performance concrete according to claim 1, characterized in that: The quartz sand includes first quartz sand, second quartz sand and third quartz sand, the particle size of the first quartz sand is less than 0.425 mm and greater than or equal to 0.25 mm, the particle size of the second quartz sand is less than 0.25 mm and greater than or equal to 0.125 mm, and the particle size of the third quartz sand is less than 0.125 mm and greater than or equal to 0.045 mm.
3. The self-compacting basalt fiber ultra-high performance concrete according to claim 2, characterized in that: The weight ratio of the first quartz sand, the second quartz sand and the third quartz sand is 29-35:18-25:30-38.
4. The self-compacting basalt fiber ultra-high performance concrete according to claim 1, characterized in that: The basalt fiber is a short-cut basalt fiber, the diameter of the short-cut basalt fiber is 17-18 μm, the length is 5-6 mm, and the density is 2.6-2.65 g / cm 3 .
5. The self-compacting basalt fiber ultra-high performance concrete according to claim 1 or 4, characterized in that: The invention comprises 3.6 to 4.14 parts of basalt fiber.
6. The self-compacting basalt fiber ultra-high performance concrete according to claim 1, characterized in that: The water reducing agent has a water reducing rate of 24% to 26%.
7. The self-compacting basalt fiber ultra-high performance concrete according to claim 1, characterized in that: The preparation method comprises the following raw materials in parts by weight: 80 parts of cement, 20 parts of silica fume, 80 parts of quartz sand, 1 part of water reducing agent, 20 parts of water and 4.14 parts of basalt fiber.
8. The self-compacting basalt fiber ultra-high performance concrete according to claim 1, characterized in that: The preparation method comprises the following raw materials in parts by weight: 75 parts of cement, 22.5 parts of silica fume, 95 parts of quartz sand, 2 parts of water reducing agent, 19 parts of water and 3.6 parts of basalt fiber.
9. The method for preparing the self-compacting basalt fiber ultra-high performance concrete according to any one of claims 1 to 8, characterized in that: The following steps are involved: After the quartz sand is mixed with cement for a first stirring, it is mixed with basalt fiber for a second stirring, and then mixed with silica fume and a water reducing agent for a third stirring, and then mixed with water for a fourth stirring to obtain a self-compacting basalt fiber ultra-high performance concrete.
10. The preparation method according to claim 9, characterized in that: The first stirring time is 30 to 50 seconds, the second stirring time is 2 to 3 minutes, the third stirring time is 1 to 2 minutes, and the fourth stirring time is 10 to 12 minutes.