Preparation and application of hydrated calcium silicate neat paste material and grouting material

By preparing hydrated calcium silicate grout at room temperature, the problem of poor compatibility between existing grouting materials and cultural relics in humid environments is solved. A porous mesh structure suitable for humid environments is provided, achieving good mechanical properties and water permeability, reducing costs and avoiding the impact of high-temperature synthesis on cultural relics.

CN118930216APending Publication Date: 2024-11-12SHANGHAI UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410997322.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-07-27
Filing Date
2024-07-24
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing grouting materials have problems in cultural relic protection, such as excessive strength, poor compatibility with the cultural relic itself, high soluble salt content, low porosity, and poor air permeability. In particular, they accelerate the weathering of stone cultural relics in humid environments, and high-temperature synthesis has a negative impact on cultural relics.

Method used

The hydrated calcium silicate grout material is formed by mixing precipitated silica, calcium hydroxide and quartz sand and curing at room temperature to form a porous network structure. It avoids the need for adding catalysts and is suitable for grouting cracks in sandstone cultural relics in humid environments.

Benefits of technology

It provides grouting materials with good mechanical strength and permeability, suitable for humid environments, reducing costs, and forming a good bond with the cultural relic, avoiding the negative impact of high-temperature synthesis on the cultural relic.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930216A_ABST
    Figure CN118930216A_ABST
Patent Text Reader

Abstract

The invention relates to preparation and application of a hydrated calcium silicate neat paste material and a grouting material. A preparation method of the hydrated calcium silicate neat paste material comprises the following steps: mixing white carbon black, calcium hydroxide and water, and curing to obtain the hydrated calcium silicate neat paste material, the preparation method of the grouting material comprises the following steps: mixing the white carbon black, the calcium hydroxide, the water and the quartz sand powder, and curing. Compared with the prior art, the requirement of the hydrated calcium silicate grouting material on the synthesis temperature is normal temperature, and the actual application requirement of cultural relic grouting materials is met; the calcium silicate hydrate grouting material still has a good reaction rate without adding a catalyst, can be synthesized in a short time and stably exists, and can realize controllable preparation of mechanical strength, components and morphology according to different strengths of a reinforced matrix; the sandstone cultural relic protection material has a porous net structure, is large in porosity, high in water absorption rate and good in water permeability, and is suitable for sandstone cultural relic protection in a humid environment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of cultural relic protection materials, and relates to the preparation and application of a calcium silicate hydrate slurry material and a grouting material, and in particular to the preparation and application of a calcium silicate hydrate slurry material and a calcium silicate hydrate grouting material for grouting cracks in sandstone cultural relic rock masses in a humid environment. Background Art

[0002] Sandstone is one of the most common rock types in my country's stone cultural relics, and sandstone cave temples account for 80% of the total number of cave temples in my country. Due to the porous characteristics of sandstone itself and the long-term influence of various factors such as human activities, surface cracks, hollows and matrix fractures have appeared. The existence of these damages, especially cracks, not only damages the strength of the rock mass of the stone cultural relics themselves, but also, under the influence of external environments such as temperature, humidity, and acidic gases, it will intensify the diffusion and migration of soluble pollutants such as acids, alkalis, and salts in the rock matrix, further accelerating the weathering of stone cultural relics, posing a great threat to the stability and preservation life of stone cultural relics.

[0003] At present, grouting is often used to protect fractures, fissures and other types of defects. Grouting technology is a method used in construction engineering to enhance the stability of buildings. This method can not only fill the huge cracks caused by geological movements, but also deal with small cracks on the surface. The grouting method can play a good role in reinforcing grotto rocks, stone carvings, etc. At the same time, the grouting method can also effectively block the seepage channels of the grottoes and play a role in controlling water leakage.

[0004] Commonly used grouting materials in the field of cultural relics protection can be divided into two categories: organic materials and inorganic materials. Organic materials include resin materials such as silicone, epoxy resin, acrylic resin, etc., which have the advantages of good permeability, fast curing, small shrinkage, and strong adhesion. However, organic materials are too strong, brittle, and have poor compatibility with the stone cultural relics after aging. They are not breathable, have a short service life, and are difficult to remove after aging.

[0005] Inorganic materials mainly include cement and hydraulic lime. The main component of cement is 3CaO·SiO 2 ,2CaO·SiO 2 、3CaO·Al 2 O 3 、4CaO·Al 2 O 3 ·Fe 2 O 3 Its curing mechanism is: ①3CaO·SiO 2 +nH 2 O→xCaO·SiO 2 ·yH 2 O+(3-x)Ca(OH)2 ;②2CaO·SiO 2 +nH 2 O→xCaO·SiO 2 ·yH 2 O+(2-x)Ca(OH) 2 ; Cement solidifies and hardens quickly, has high strength, is frost-resistant and durable, and shrinks little when dried, making it suitable for the reinforcement of dangerous rock masses; however, the application of cement in cultural relics protection has always been controversial, mainly due to its excessive strength, poor compatibility with the cultural relics themselves, high soluble salt content after use, low porosity, poor air permeability, large differences in mechanical strength and thermal expansion coefficient from the stone matrix, and even damage to the cultural relics themselves.

[0006] Hydraulic lime has been used in Europe for a long time. It has been used to repair old stone buildings since the mid-19th century. Its curing is mainly divided into the following two stages: ① Dicalcium silicate hydration: 2CaO·SiO 2 +nH 2 O=nCaO·SiO 2 ·yH 2 O+(2-x)Ca(OH) 2 ②Ca(OH) 2 Carbonization: Ca(OH) 2 +CO 2 =CaCO 3 +H 2 O. The solidified product of hydraulic lime has moderate strength, good compatibility with the substrate to be repaired, especially limestone, marble, etc., strong anti-pollution ability, low soluble salt content, and good water permeability. However, the current use of hydraulic lime in China mainly relies on imports, which is costly and in low supply, so its large-scale application is limited.

[0007] Calcium silicate hydrate is the main solidification product of cement and hydraulic lime, and is the main source of the mechanical properties of cement and hydraulic lime. Therefore, choosing raw materials with wide sources and low prices to artificially synthesize calcium silicate hydrate and adding aggregates and additives to make relatively pure calcium silicate hydrate grouting materials can ensure that while having good performance, no soluble salts are introduced into cultural relics and meet the needs of large-scale applications. Summary of the invention

[0008] The purpose of the present invention is to provide a preparation method and application of a calcium silicate hydrate slurry material and a calcium silicate hydrate grouting material for grouting cracks in sandstone cultural relics in a humid environment. The calcium silicate hydrate grouting material is a hydraulic material with a composition similar to that of the cultural relic body, good mechanical strength and controllable. It has a porous mesh structure, a large porosity, and good water permeability, and is suitable for grouting cracks in sandstone cultural relics in a humid environment; the raw material cost is low, and volcanic ash reaction can quickly occur at room temperature without adding any catalyst to generate calcium silicate hydrate, which greatly simplifies the synthesis steps, and the physical phase in the final product is simple, mainly amorphous calcium silicate hydrate.

[0009] The purpose of the present invention can be achieved by the following technical solutions:

[0010] A method for preparing a calcium silicate hydrate slurry material comprises: mixing and solidifying white carbon black, calcium hydroxide and water to obtain the calcium silicate hydrate slurry material, wherein no catalyst is added.

[0011] Furthermore, the molar ratio of calcium to silicon in the white carbon black and calcium hydroxide is (0.8-1.5):1.

[0012] Furthermore, the water-solid ratio of the raw material is (1.8-2.2):1, wherein the solids are white carbon black and calcium hydroxide.

[0013] Furthermore, the curing is carried out at room temperature and the curing time is 26 to 30 days.

[0014] A method for preparing a calcium silicate hydrate grouting material comprises: mixing white carbon black, calcium hydroxide, water and quartz sand powder, and curing and solidifying to obtain the calcium silicate hydrate grouting material.

[0015] Furthermore, the molar ratio of calcium to silicon in the white carbon black and calcium hydroxide is (0.8-1.5):1.

[0016] Furthermore, the water-solid ratio of the raw material is (1.8-2.2):1, wherein the solids are white carbon black and calcium hydroxide.

[0017] Furthermore, the ratio of the mass of the quartz sand powder to the total mass of white carbon black and calcium hydroxide is (2.5-3.5):1.

[0018] Furthermore, the curing and curing is carried out in a closed environment, the curing temperature is 15-25° C., and the curing time is 26-30 days. The closed environment can be achieved by completely wrapping the material with plastic wrap.

[0019] Furthermore, the method further comprises adding a polycarboxylate water reducer, wherein the added amount is preferably 4% of the total mass of white carbon black and calcium hydroxide.

[0020] An application of a calcium silicate hydrate grout material includes using the calcium silicate hydrate grout material for grouting cracks in a sandstone cultural relic rock mass in a humid environment. The calcium silicate hydrate grout material of the present invention can be synthesized in situ inside the cultural relic under normal temperature conditions, thereby avoiding the negative impact of high-temperature synthesis conditions on the cultural relic in the prior art.

[0021] Compared with the prior art, the present invention has the following characteristics:

[0022] The calcium silicate hydrate grouting material prepared by the present invention and used for grouting cracks in sandstone cultural relics in a humid environment has a requirement for the synthesis temperature of room temperature, which meets the actual application requirements of the cultural relics grouting material; it has a good reaction rate without adding a catalyst, can synthesize the calcium silicate hydrate grouting material with a simple phase, high purity and good mechanical properties in a relatively short time and stably exist, and can also realize controllable preparation of mechanical strength, composition and morphology according to the different strengths of the reinforced matrix; it has a porous network structure, a large porosity, a high water absorption rate and good water permeability, and is suitable for the protection of sandstone cultural relics in a humid environment. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is a macroscopic picture of the calcium silicate hydrate slurry material prepared by the present invention;

[0024] Figure 2 X-ray diffraction patterns of calcium silicate hydrate slurry materials obtained by reacting for 28 days under the conditions of calcium-silicon molar ratios of 0.8, 1.0, 1.2, 1.5, and 2.0 in Examples 1, 2, 3, 4, and Comparative Example 1, respectively;

[0025] Figure 3 The SEM images of calcium silicate hydrate slurry materials obtained by reacting for 28 days under the conditions of calcium-silicon molar ratios of 0.8, 1.0, 1.2, 1.5, and 2.0, respectively, in Examples 1, 2, 3, 4, and Comparative Example 1;

[0026] Figure 4 The X-ray diffraction patterns of the calcium silicate hydrate slurry material obtained by curing for 1 and 3 days at a calcium-silicon ratio of 0.8 in Comparative Example 2;

[0027] Figure 5 This is the X-ray diffraction spectrum of the calcium silicate hydrate slurry material obtained by curing for 1 and 3 days at room temperature under comparative example 3 with a calcium-silicon molar ratio of 0.8 and a certain amount of catalyst added.

[0028] Figure 6 This is a macroscopic picture of the sample of the calcium silicate hydrate grouting material consolidation 28 days in Example 5;

[0029] Figure 7The X-ray diffraction patterns of the solidified calcium silicate grouting materials obtained by reacting for 28 days under the conditions of calcium-silicon molar ratios of 0.8, 1.0, 1.2, and 1.5, respectively, in Examples 5, 6, 7, and 8;

[0030] Figure 8 The flexural and compressive strengths of the calcium silicate hydrate grouting material consolidation products obtained at 28 days in Examples 5, 6, 7, and 8 under the conditions where the calcium-silicon molar ratio is 0.8, 1.0, 1.2, and 1.5 respectively;

[0031] Fig. 9 The flexural and compressive strengths of the calcium silicate hydrate grouting material concretions obtained by reacting for 28 days under the conditions of 0%, 4%, 3% and 5% addition of high-performance polycarboxylate water-reducing agent in Examples 5 and 9 and Comparative Examples 4 and 5.

[0032] Fig.10 The flexural and compressive strengths of the calcium silicate hydrate grouting material solids obtained by reacting for 28 days under the conditions of deionized water and cementitious material (white carbon black, calcium hydroxide) mass ratios of 2.0, 1.5, and 2.5 in Example 9 and Comparative Examples 6 and 7. DETAILED DESCRIPTION

[0033] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.

[0034] The calcium silicate hydrate grouting material for grouting cracks in sandstone cultural relics in a humid environment provided by the present invention is prepared based on a volcanic ash reaction method. The volcanic ash reaction method refers to a certain amount of active components, such as active silicon dioxide, in certain volcanic ash mixtures, which react with calcium hydroxide to generate a reaction product, calcium silicate hydrate.

[0035] The following is an exemplary description of the preparation method of the calcium silicate hydrate grouting material, which comprises the following steps: mixing white carbon black, calcium hydroxide and a certain amount of water evenly at room temperature under magnetic stirring, and then curing at room temperature in a closed environment to obtain a calcium silicate hydrate slurry material. On the basis of the preparation of the calcium silicate hydrate slurry material, quartz sand and high-performance polycarboxylic acid water-reducing agent are added to finally prepare the calcium silicate hydrate grouting material with excellent performance. All reactions are performed at room temperature by default, and no catalyst is added.

[0036] In the above preparation process, the main chemical reactions are as follows: xCa(OH) 2 +ySiO 2 +(zx)H 2 O=xCaO-ySiO 2 -zH 2 O. The reaction parameter of calcium-silicon molar ratio can be regulated by controlling the amount of white carbon black and calcium hydroxide added in the raw materials.

[0037] In some embodiments, the white carbon black may be amorphous nano-silicon dioxide; amorphous silicon dioxide with a nano-particle size has a larger specific surface area and greater reaction activity, and can fully react with calcium hydroxide to produce a volcanic ash reaction to synthesize a hydrated calcium silicate material.

[0038] In some embodiments, the calcium hydroxide has an average particle size of 500 nm and a purity of ≥95 wt.%.

[0039] In some embodiments, the calcium-silicon (Ca / Si) molar ratio of the raw material can be controlled to be 0.8-1.5. The calcium-silicon molar ratio determines the structure and morphology of the calcium silicate hydrate material. Experiments have found that: at room temperature and a constant water-solid ratio, when the calcium-silicon ratio is in the range of 0.8-1.5, the raw material can be completely converted into calcium silicate hydrate; when the calcium-silicon molar ratio is 0.8, the morphology of the generated calcium silicate hydrate is a layered stacking structure, and when the calcium-silicon molar ratio is in the range of 1.0-1.5, the layered structure gradually transforms into a foil-like structure.

[0040] In some embodiments, the water-to-solid ratio is controlled to be 2:1, that is, the mass ratio of deionized water to cementitious material (white carbon black, calcium hydroxide) is 2:1. When the water-to-solid ratio is lower than 2:1, it is difficult for the raw materials to obtain fluidity; when the water-to-solid ratio is above 2:1, a hydrated calcium silicate material can be generated, and the reaction rate is relatively fast. On the third day of the reaction, the raw materials are almost completely converted into hydrated calcium silicate. And when the calcium-silicon molar ratio remains constant, the morphology of the hydrated calcium silicate materials generated by different water-to-solid ratios is similar. Considering the erosive effect of water on sandstone cultural relics, the water content of the raw materials cannot be too high. Therefore, the water-to-solid ratio is controlled to 2:1, which can not only obtain a hydrated calcium silicate material with good fluidity, but also minimize the destructive effects of water on sandstone cultural relics.

[0041] In some embodiments, the rotation speed of the magnetic stirring may be 1000 rpm, so that the raw materials are evenly mixed.

[0042] In some embodiments, the curing time at room temperature may be 28 days. Since white carbon black has a small particle size and a large specific surface area, it has good reactivity. At the 28th day, the raw materials have been completely converted into calcium silicate hydrate.

[0043] Compared with calcium silicate hydrate paste with only cementitious material, adding a certain amount of quartz sand can obtain better mechanical properties and reduce the amount of cementitious material, thereby reducing costs, so it is widely used in practical engineering. In some embodiments, the mass ratio of quartz sand to cementitious material (white carbon black, calcium hydroxide) can be controlled to 3:1 to obtain good mechanical strength.

[0044] High-performance polycarboxylate water-reducing agent improves the fluidity of grouting materials and reduces the amount of water used by reducing the intermolecular forces. The appropriate amount of water-reducing agent plays a vital role in the final grouting effect of the grouting material. In some embodiments, the amount of the high-performance polycarboxylate water-reducing agent added can be controlled to be 4wt.% of the total mass of white carbon black and calcium hydroxide. When the content of high-performance polycarboxylate water-reducing agent is lower than 4wt.%, the fluidity of the calcium silicate hydrate grouting material is poor, which will cause the material to be unable to enter the internal cracks of sandstone cultural relics to play a reinforcing and bonding role in practical applications; when the content of polycarboxylate water-reducing agent accounts for more than 4wt.%, it will affect the development of material strength and reduce the purity of the synthesized calcium silicate hydrate. In order to ensure the mechanical strength and purity of the calcium silicate hydrate grouting material, it is necessary to set the addition ratio of the high-performance polycarboxylate water-reducing agent to 4wt.%.

[0045] The calcium silicate hydrate grouting material obtained by the preparation method provided by the present invention has good mechanical strength, can still maintain good performance in water, has strong water resistance, and is suitable for the protection of sandstone cultural relics in humid environments. The microscopic morphology of the calcium silicate hydrate grouting material prepared by the present invention is a porous network structure, which can form a good bonding effect with the cultural relic body.

[0046] The present invention proposes for the first time to synthesize relatively pure calcium silicate hydrate for use as a protective material for grouting cracks in sandstone cultural relics in a humid environment. In addition, the present invention imitates the environmental characteristic of lack of carbon dioxide in the cracks inside the rock mass, and adopts a curing method of covering the surface of the grouting material with plastic wrap. This curing method effectively avoids the reaction between carbon dioxide in the air and calcium hydroxide, promotes the synthesis of calcium silicate hydrate, and finally obtains a calcium silicate hydrate grouting material with a high purity, which provides a new idea for the application of materials such as hydraulic lime in the grouting of cracks in sandstone rock mass.

[0047] The following embodiments are implemented based on the above technical solution of the present invention, and provide detailed implementation methods and specific operation processes, but the protection scope of the present invention is not limited to the following embodiments.

[0048] Embodiment 1:

[0049] Weigh about 10 g each of white carbon black (purchased from Henan Baihong Chemical Products Sales Co., Ltd.) and calcium hydroxide (purchased from Shanghai McLean Biochemical Technology Co., Ltd.) and 40 g of deionized water, select some of them as raw materials, control the calcium-silicon molar ratio of the raw materials to 0.8, and the water-solid ratio of the raw materials to 2:1.

[0050] Add white carbon black and calcium hydroxide into a beaker and mix well. Then add deionized water. Place the mixture on a magnetic stirrer and stir well. Set the speed to 1000 rpm.

[0051] After standing for 28 days at room temperature to solidify, a calcium silicate hydrate slurry material was obtained. Figure 1 shown.

[0052] In order to facilitate the characterization of the microscopic composition and morphology of calcium silicate hydrate, the prepared calcium silicate hydrate slurry material was vacuum filtered and ground to obtain calcium silicate hydrate powder. The calcium silicate hydrate material prepared in Example 1 is recorded as A, and the microscopic morphology and structure of the obtained calcium silicate hydrate are characterized by XRD and SEM, and TGA-DSC is used to judge the mass loss and heat absorption or release of the synthetic material with temperature changes, indicating that the calcium silicate hydrate material can be synthesized using this inventive method.

[0053] Example 2

[0054] The preparation method of this embodiment is the same as that of embodiment 1, except that the molar ratio of calcium to silicon is 1.0. The rest is the same as that of embodiment 1.

[0055] The calcium silicate hydrate material obtained in Example 2 is denoted as B, and its microscopic morphology and structure are characterized by XRD and SEM. TGA-DSC is used to determine the mass loss and heat absorption or release of the synthetic material as the temperature changes, indicating that the calcium silicate hydrate material can be synthesized using this inventive method.

[0056] Example 3

[0057] The preparation method of this embodiment is the same as that of embodiment 1, except that the molar ratio of calcium to silicon is 1.2. The rest is the same as that of embodiment 1.

[0058] The calcium silicate hydrate material obtained in Example 3 is denoted as C, and its microscopic morphology and structure are characterized by XRD and SEM. TGA-DSC is used to determine the mass loss and heat absorption or release of the synthetic material as the temperature changes, indicating that the calcium silicate hydrate material can be synthesized using this inventive method.

[0059] Example 4

[0060] The preparation method of this embodiment is the same as that of embodiment 1, except that the molar ratio of calcium to silicon is 1.5. The rest is the same as that of embodiment 1.

[0061] The calcium silicate hydrate material obtained in Example 4 is denoted as D, and its microscopic morphology and structure are characterized by XRD and SEM. TGA-DSC is used to determine the mass loss and heat absorption or release of the synthetic material as the temperature changes, indicating that the calcium silicate hydrate material can be synthesized using this inventive method.

[0062] Comparative Example 1

[0063] The preparation method of this embodiment is the same as that of embodiment 1, except that the molar ratio of calcium to silicon is 2.0. The rest is the same as that of embodiment 1.

[0064] The material prepared in Comparative Example 1 was recorded as E, and its composition and morphology were characterized by XRD, SEM, and TGA-DSC. It was found that the raw materials of the synthesis method could not be completely reacted to form calcium silicate hydrate material, and a large amount of calcium hydroxide remained in the system, indicating that under the reaction condition of a calcium-silicon molar ratio of 2.0, calcium hydroxide was excessive.

[0065] Figure 2 The XRD diagrams of calcium silicate hydrate slurry materials obtained by reacting for 28 days under different calcium-silicon molar ratios of Examples 1, 2, 3, 4 and Comparative Example 1 are as follows. It can be seen from the diagram that when the calcium-silicon molar ratio is 0.8, 1.0, 1.2, and 1.5, the raw materials can all be completely reacted to form calcium silicate hydrate; when the calcium-silicon molar ratio is 2.0, there is obvious excess calcium hydroxide.

[0066] Figure 3 The SEM images of the calcium silicate hydrate slurry materials obtained by reacting for 28 days under different calcium-silicon molar ratios of Examples 1, 2, 3, 4 and Comparative Example 1 are shown. When the calcium-silicon molar ratio is 0.8, the calcium silicate hydrate mainly presents irregular, amorphous stacking, and the stacking structure is relatively dense. As the calcium-silicon molar ratio increases, foil-like calcium silicate hydrate appears and gradually increases. When the calcium-silicon molar ratio is 2.0, the foil-like calcium silicate hydrate is surrounded by unreacted calcium hydroxide.

[0067] Comparative Example 2:

[0068] The preparation method of this embodiment is the same as that of embodiment 1, except that the samples are taken after curing for 1 and 3 days, that is, the samples are taken after standing at room temperature for 1 and 3 days to cure.

[0069] The calcium silicate hydrate material obtained in Comparative Example 2 is denoted as F, and the formation of calcium silicate hydrate is characterized by XRD. The rate of volcanic ash reaction within 3 days is tested by microcalorimeter, indicating that the method of the invention can synthesize a large amount of calcium silicate hydrate material in a short time.

[0070] Figure 4 The XRD patterns of the calcium silicate hydrate slurry material obtained in Comparative Example 2 at room temperature and with a calcium-silicon molar ratio of 0.8 after 1 and 3 days of reaction are shown in the graph. It can be seen from the graph that calcium silicate hydrate is generated after 1 day of reaction, but there is also obvious residual calcium hydroxide; after 3 days, a large amount of calcium silicate hydrate is generated, and there is no obvious residual calcium hydroxide. This indicates that the volcanic ash reaction has been relatively complete on the 3rd day.

[0071] Comparative Example 3:

[0072] The preparation method of this embodiment refers to Comparative Example 2, except that 0.03% of the total weight of calcium hydroxide, white carbon black and deionized water is added as a catalyst for the reaction. The rest is the same as Comparative Example 2.

[0073] The calcium silicate hydrate material obtained in Comparative Example 3 is denoted as F', and the generation of the calcium silicate hydrate is characterized by XRD.

[0074] Figure 5 This is the XRD pattern of the calcium silicate hydrate slurry material obtained by reaction 1 and 3d under room temperature conditions with a calcium-silicon molar ratio of 0.8 and a certain amount of catalyst added in Comparative Example 3. It can be seen from the spectrum that compared with the comparative example 2 test group without adding a catalyst, whether or not the catalyst is added has almost no effect on the synthesis rate of calcium silicate hydrate, which confirms that a sufficient amount of calcium silicate hydrate can be obtained without using a catalyst.

[0075] Embodiment 5:

[0076] Weigh 120g each of white carbon black and calcium hydroxide, add them to a planetary shaft mixer, first manually stir the dry materials evenly, and then add 480g of deionized water. Stir slowly for 1 minute and then stop. Scrape off the slurry on the mixer blades and the container wall, then stir quickly for 1 minute and stop. Then add 720g of quartz sand powder, stir slowly for 1 minute, then stir quickly for 1 minute and stop. Pour the evenly mixed mortar into a 40mm×40mm×160mm mold and wrap it with plastic wrap to reduce the carbonization reaction of calcium hydroxide in the mortar with carbon dioxide in the air. Three parallel samples are prepared for one set of experimental formulas. The mold is then placed in a curing box at 20°C and 90% RH for 28 days and then demolded to obtain a sample of calcium silicate hydrate grouting material after curing for 28 days. Figure 4 The calcium-silicon molar ratio of the cementitious material (white carbon black and calcium hydroxide) is controlled to be 0.8, the mass ratio of deionized water to the cementitious material (white carbon black and calcium hydroxide) is 2:1, and the mass ratio of quartz sand to the cementitious material is 3:1.

[0077] The calcium silicate hydrate grouting material prepared in Example 5 is denoted as G, and its consolidated body is subjected to flexural and compressive tests using a universal testing machine to obtain the flexural and compressive strengths of the calcium silicate hydrate grouting material. In order to facilitate the characterization of the microscopic composition and morphology of the calcium silicate hydrate grouting material, a small amount of the calcium silicate hydrate grouting material consolidated material is filtered and dried to obtain calcium silicate hydrate powder. The obtained calcium silicate hydrate powder is characterized by XRD and SEM for its microscopic morphology and structure.

[0078] Embodiment 6:

[0079] The preparation method of this embodiment refers to that of embodiment 5, except that the molar ratio of calcium to silicon is 1.0. The rest is the same as that of embodiment 5.

[0080] The calcium silicate hydrate grouting material prepared in Example 6 is denoted as H, and its consolidated body is subjected to flexural and compressive tests using a universal testing machine to obtain the flexural and compressive strengths of the calcium silicate hydrate grouting material. In order to facilitate the characterization of the microscopic composition and morphology of the calcium silicate hydrate grouting material, a small amount of the calcium silicate hydrate grouting material consolidated material is filtered and dried to obtain calcium silicate hydrate powder. The obtained calcium silicate hydrate powder is characterized by XRD and SEM for its microscopic morphology and structure.

[0081] Embodiment 7:

[0082] The preparation method of this embodiment is the same as that of embodiment 5, except that the molar ratio of calcium to silicon is 1.2. The rest is the same as that of embodiment 5.

[0083] The calcium silicate hydrate grouting material prepared in Example 7 is denoted as I, and its consolidated body is subjected to flexural and compressive tests using a universal testing machine to obtain the flexural and compressive strengths of the calcium silicate hydrate grouting material. In order to facilitate the characterization of the microscopic composition and morphology of the calcium silicate hydrate grouting material, a small amount of the calcium silicate hydrate grouting material consolidated material is filtered and dried to obtain calcium silicate hydrate powder. The obtained calcium silicate hydrate powder is characterized by XRD and SEM for its microscopic morphology and structure.

[0084] Embodiment 8:

[0085] The preparation method of this embodiment refers to that of embodiment 5, except that the molar ratio of calcium to silicon is 1.5. The rest is the same as that of embodiment 5.

[0086] The calcium silicate hydrate grouting material prepared in Example 8 is denoted as J. The flexural and compressive tests are performed on the consolidated body using a universal testing machine to obtain the flexural and compressive strengths of the calcium silicate hydrate grouting material. In order to facilitate the characterization of the microscopic composition and morphology of the calcium silicate hydrate grouting material, a small amount of the consolidated material of the calcium silicate hydrate grouting material is filtered and dried to obtain a calcium silicate hydrate powder. The obtained calcium silicate hydrate powder is characterized by XRD and SEM for its microscopic morphology and structure.

[0087] Figure 7 The XRD diagrams of the calcium silicate hydrate grouting materials obtained by reacting for 28 days under the conditions of calcium-silicon molar ratios of 0.8, 1.0, 1.2 and 1.5 in Examples 5, 6, 7 and 8 show that when the calcium-silicon molar ratio is 0.8, 1.0, 1.2 and 1.5, the raw materials can completely react to form calcium silicate hydrate, and there is no obvious calcium hydroxide remaining in the system.

[0088] Figure 8The flexural and compressive strengths of the calcium silicate grouting material consolidation obtained by reacting for 28 days under the conditions of calcium-silicon molar ratios of 0.8, 1.0, 1.2, and 1.5 in Examples 5, 6, 7, and 8, respectively. The calcium silicate grouting material consolidation obtained under different calcium-silicon molar ratios all have good mechanical strength. As the calcium-silicon molar ratio increases, the mechanical strength gradually decreases.

[0089] Embodiment 9:

[0090] The preparation method of this embodiment refers to that of embodiment 5, except that a high-performance polycarboxylate water-reducing agent (purchased from Shanghai Chenqi Chemical Technology Co., Ltd.) is added, and the amount of the high-performance polycarboxylate water-reducing agent added is 4 wt.% of the mass of the cementitious material, i.e., 9.6 g. The rest is the same as that of embodiment 5.

[0091] The calcium silicate hydrate grouting material prepared in Example 9 is denoted as K. The fluidity of fresh slurry is tested with a cement paste fluidity test mold. It can be found that the average fluidity of the slurry is 259±3 mm. It can be considered that the grouting material has good fluidity.

[0092] The flexural and compressive strengths of the consolidated body were tested by a universal testing machine to obtain the flexural and compressive strengths of the calcium silicate hydrate grouting material.

[0093] Comparative Example 4:

[0094] The preparation method of this embodiment is the same as that of embodiment 9, except that the amount of high-performance polycarboxylate water-reducing agent added is 3 wt.% of the mass of the cementitious material, i.e., 7.2 g. The rest is the same as that of embodiment 9.

[0095] The calcium silicate hydrate grouting material prepared in Comparative Example 4 is denoted as L. The fluidity of the fresh slurry is tested with a cement slurry fluidity test mold. It can be found that the average fluidity of the slurry is 145±2 mm, which means there is almost no fluidity.

[0096] The flexural and compressive strengths of the consolidated body were tested by a universal testing machine to obtain the flexural and compressive strengths of the calcium silicate hydrate grouting material.

[0097] Comparative Example 5:

[0098] The preparation method of this embodiment is the same as that of embodiment 9, except that the amount of high-performance polycarboxylate water-reducing agent added is 5wt.% of the mass of the cementitious material, that is, 12g. The rest is the same as that of embodiment 9.

[0099] The calcium silicate hydrate grouting material prepared in Comparative Example 5 is denoted as M. The fluidity of the fresh slurry is tested with a cement slurry fluidity test mold. It can be found that the average fluidity of the slurry is 264±3 mm, and the fluidity is good.

[0100] The flexural and compressive strengths of the consolidated body were tested by a universal testing machine to obtain the flexural and compressive strengths of the calcium silicate hydrate grouting material.

[0101] Fig. 9 The flexural and compressive strengths of the calcium silicate hydrate grouting material concretions obtained by reacting for 28 days under the conditions of 0wt.%, 4wt.%, 3wt.%, and 5wt.% addition of the high-performance polycarboxylate water-reducing agent in Examples 5 and 9 and Comparative Examples 4 and 5. When the addition amount of the high-performance polycarboxylate water-reducing agent is greater than or equal to 4wt.%, the mechanical properties of the calcium silicate hydrate grouting material are significantly improved.

[0102] Comparative Example 6:

[0103] The preparation method of this embodiment refers to that of embodiment 9, except that the mass ratio of deionized water to gelling material (white carbon black and calcium hydroxide) is 1.5:1. The rest is the same as that of embodiment 9.

[0104] The calcium silicate hydrate grouting material prepared in Comparative Example 6 is denoted as N. The fluidity of the fresh slurry is tested with a cement paste fluidity test mold, and it is found that the slurry has almost no fluidity.

[0105] The flexural and compressive strengths of the consolidated body were tested by a universal testing machine to obtain the flexural and compressive strengths of the calcium silicate hydrate grouting material.

[0106] Comparative Example 7:

[0107] The preparation method of this embodiment refers to that of embodiment 9, except that the mass ratio of deionized water to gelling material (white carbon black and calcium hydroxide) is 2.5:1. The rest is the same as that of embodiment 9.

[0108] The calcium silicate hydrate grouting material prepared in Comparative Example 7 is denoted as O. The fluidity of the fresh slurry is tested with a cement slurry fluidity test mold. It can be found that the average fluidity of the slurry is 295±2 mm, and the fluidity is good.

[0109] The flexural and compressive strengths of the consolidated body were tested by a universal testing machine to obtain the flexural and compressive strengths of the calcium silicate hydrate grouting material.

[0110] Fig.10 The flexural and compressive strengths of the calcium silicate hydrate grouting material solids obtained by reacting for 28 days under the conditions of the mass ratio of deionized water to cementitious material (white carbon black, calcium hydroxide) of Example 9 and Comparative Examples 6 and 7 at 2.0, 1.5, and 2.5. Although the mechanical properties are good when the water-to-solid ratio is 1.5, the formula has no practical application value due to its poor fluidity.

[0111] The present invention can draw the following conclusions: white carbon black has good reaction activity, and a large amount of calcium silicate hydrate can be generated in only 3 days under normal temperature conditions; when the calcium-silicon molar ratio is 0.8, 1.0, 1.2, and 1.5, the raw materials can be completely converted into calcium silicate hydrate after curing for 28 days; with the increase of the calcium-silicon molar ratio, the mechanical strength of the consolidated body of the calcium silicate hydrate grouting material shows a downward trend; when the high-performance polycarboxylate water-reducing agent is added in an amount greater than or equal to 4wt.% of the mass of the cementitious material, the mechanical properties of the calcium silicate hydrate grouting material are significantly improved. When the mass ratio of deionized water to cementitious material (white carbon black, calcium hydroxide) is 2.0, both fluidity and good mechanical properties can be taken into account.

[0112] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.

Claims

1. A method for preparing a calcium silicate hydrate slurry material, characterized in that: include: The white carbon black, calcium hydroxide and water are mixed and solidified to obtain a hydrated calcium silicate slurry material.

2. The method for preparing the calcium silicate hydrate slurry material according to claim 1, characterized in that: The molar ratio of calcium to silicon in the white carbon black and calcium hydroxide is (0.8-1.5):

1.

3. The method for preparing the calcium silicate hydrate slurry material according to claim 1, characterized in that: The water-solid ratio of the raw materials is (1.8-2.2):1, wherein the solids are white carbon black and calcium hydroxide.

4. The method for preparing the calcium silicate hydrate slurry material according to claim 1, characterized in that: Curing is carried out at room temperature and the curing time is 26 to 30 days.

5. A method for preparing a calcium silicate hydrate grouting material, characterized in that: include: The calcium silicate hydrate grouting material is obtained by mixing white carbon black, calcium hydroxide, water and quartz sand powder, and curing and solidifying.

6. The method for preparing the calcium silicate hydrate grouting material according to claim 5, characterized in that: The molar ratio of calcium to silicon in the white carbon black and calcium hydroxide is (0.8-1.5):1; the water-solid ratio of the raw materials is (1.8-2.2):1, wherein the solids are white carbon black and calcium hydroxide.

7. The method for preparing the calcium silicate hydrate grouting material according to claim 5, characterized in that: The ratio of the mass of the quartz sand powder to the total mass of white carbon black and calcium hydroxide is (2.5-3.5):

1.

8. The method for preparing the calcium silicate hydrate grouting material according to claim 5, characterized in that: Curing and curing are carried out in a closed environment, the curing temperature is 15-25°C, and the curing time is 26-30 days.

9. The method for preparing the calcium silicate hydrate grouting material according to claim 5, characterized in that: It also includes adding polycarboxylate water reducer.

10. An application of the calcium silicate hydrate grouting material prepared by the method according to claim 5, characterized in that: The calcium silicate hydrate grouting material is used for grouting cracks in sandstone cultural relics rock mass in a humid environment.

Citation Information

Cited By

  • High-activity beta-Ca2SiO4 for cultural relic protection and preparation and application thereof