High-temperature-resistant heat-insulating aerogel and preparation method thereof

By adding L-phenylalanine and graphene oxide to the silica aerogel, the modified sol and infiltrate the fiber preforms, the problem of poor thermal insulation performance of traditional aerogels at high temperatures is solved, and the problem of poor thermal insulation performance of traditional aerogels is achieved. High-temperature insulation aerogel with high porosity, low density and low thermal conductivity is suitable for industrial production.

CN118930219AActive Publication Date: 2024-11-12吉祥三宝高科新材料有限公司
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410992613.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-12
Estimated Expiration
2044-07-23

AI Technical Summary

Technical Problem

Traditional silica aerogel materials have poor thermal insulation performance at high temperatures and are prone to adsorbing water vapor in humid environments, resulting in an increase in thermal conductivity, limiting their application range.

Method used

The modified sol was prepared by acid-base two-step catalytic method using L-phenylalanine and graphene oxide as modifiers, and penetrated into the fiber prefabricated parts, and obtained resistance by vacuum pressurized impregnation, aging, drying and sintering. High temperature thermal insulation aerogel.

Benefits of technology

Under 1100°C, the thermal conductivity of the aerogel is 0.030-0.035W/(m·K), and has excellent thermal insulation properties. It is simple in preparation and low in cost, which is suitable for large-scale industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004959268790000061
    Figure BDA0004959268790000061
Patent Text Reader

Abstract

The invention discloses high-temperature-resistant heat-insulating aerogel and a preparation method thereof, and belongs to the technical field of aerogel. The preparation method of the high-temperature-resistant heat-insulating aerogel comprises the following steps: firstly, adding L-phenylalanine and graphene oxide into deionized water, performing ultrasonic dispersion, adjusting the pH value, heating and stirring, cooling and dialyzing, and freeze-drying to obtain modified graphene oxide; mixing a silicon source, absolute ethyl alcohol and acid, and stirring at room temperature to obtain a precursor solution; dissolving the modified graphene oxide in absolute ethyl alcohol, performing ultrasonic dispersion, mixing with the precursor solution, adding alkali, and continuously stirring to obtain sol; pressing the fibers into a fiber prefabricated part; immersing the obtained fiber prefabricated member into the sol, vacuumizing and maintaining the pressure, and recovering to normal pressure to obtain a fiber and sol composite material; and finally, aging, drying and sintering the fiber and sol composite material to obtain the high-temperature-resistant heat-insulating aerogel.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of aerogels, and in particular relates to a high temperature resistant heat insulating aerogel and a preparation method thereof. Background Art

[0002] Aerogel is an ultra-light solid material with a continuous three-dimensional network structure. According to the differences in its structural components, it is divided into three categories: inorganic aerogel, organic aerogel and carbon aerogel. Aerogel has the characteristics of high porosity, high specific surface area, low density, low thermal conductivity, low elastic modulus, strong adsorption, low refractive index, low acoustic impedance, etc., which makes it have broad application prospects in many fields such as mechanics, thermodynamics, optics, acoustics, etc.

[0003] Silica aerogel is one of the aerogels with relatively perfect preparation technology. It is widely recognized and praised by the thermal insulation material industry for its good physical and chemical properties and ultra-low thermal conductivity. However, the traditional single-system SiO2 aerogel material can only withstand a temperature of 600°C, which greatly limits the application range of the material. In addition, silica aerogel is hydrophilic due to its porous characteristics and the presence of a large number of hydroxyl groups (-OH) on the surface. It easily absorbs water vapor in a humid environment, resulting in increased thermal conductivity and decreased thermal insulation performance. Therefore, the research of aerogel materials with good thermal insulation and high temperature resistance is a problem that needs to be solved at present. Summary of the invention

[0004] The object of the present invention is to provide a high temperature resistant heat insulating aerogel and a preparation method thereof, so as to solve the problem that the heat insulating performance of the aerogel is poor.

[0005] The purpose of the present invention can be achieved through the following technical solutions:

[0006] A method for preparing a high temperature resistant heat insulating aerogel comprises the following steps:

[0007] Step 1, adding L-phenylalanine and graphene oxide into deionized water, ultrasonically dispersing, adjusting the pH to 10-10.2, stirring at 90-95° C., cooling and dialysis, and freeze-drying to obtain modified graphene oxide;

[0008] Step 2, mixing a silicon source, anhydrous ethanol and an acid, and stirring at room temperature to obtain a precursor solution; dissolving the modified graphene oxide in anhydrous ethanol, mixing with the precursor solution after ultrasonic dispersion, adding a base and continuing stirring to obtain a sol;

[0009] Step 3, pressing the fibers into a fiber preform;

[0010] Step 4, immersing the fiber preform obtained in step 3 into the sol obtained in step 2, evacuating to -0.09 to -0.1 MPa, maintaining the pressure for 2 to 3 hours, and returning the pressure to normal pressure by introducing air to obtain a fiber and sol composite material;

[0011] Step 5: ageing, drying and sintering the fiber and sol composite material to obtain a high temperature resistant heat insulating aerogel.

[0012] Furthermore, in step 1, the dosage ratio of L-phenylalanine, graphene oxide and deionized water is 0.2-0.4 g: 1 g: 100 mL.

[0013] Furthermore, in step 2, the usage ratio of silicon source, anhydrous ethanol, acid and base is 8-10 g: 250 mL: 0.02 mL: 0.1 mL; the usage ratio of modified graphene oxide and anhydrous ethanol is 0.3-0.5 g: 100 mL.

[0014] Furthermore, graphene oxide is prepared by Hummers method.

[0015] Furthermore, the silicon source is one of ethyl orthosilicate and methyl orthosilicate.

[0016] Furthermore, the acid is one of nitric acid, hydrochloric acid and sulfuric acid.

[0017] Furthermore, the base is aqueous ammonia.

[0018] Furthermore, the fiber is one of zirconia fiber, alumina fiber, quartz fiber and mullite fiber.

[0019] A high temperature resistant heat insulating aerogel is prepared by the above steps.

[0020] Beneficial effects of the present invention:

[0021] The high temperature resistant heat insulating aerogel of the present invention has not only high porosity, but also low density and thermal conductivity, and the thermal conductivity is 0.030-0.035 W / (m·K) at 1100° C. It can be seen that the aerogel obtained in the present invention has excellent heat insulating properties.

[0022] The high temperature resistant heat insulating aerogel provided by the present invention uses an organic silicon source as a precursor, adds modified graphene oxide aerogel, utilizes an acid-base two-step catalytic method to prepare a modified sol, and infiltrates the modified silica sol into a fiber preform by vacuum pressure impregnation to obtain a fiber and sol composite material. After gel aging, drying, and sintering, a high temperature resistant heat insulating aerogel is finally obtained. The preparation method is simple, low in cost, and suitable for large-scale industrial production.

[0023] The modified graphene oxide prepared in the present invention firstly adopts the Hummers method to prepare graphene oxide with high specific surface area, and then L-phenylalanine is used as a hydrophobic modifier to prepare graphene oxide aerogel with high hydrophobicity. After being mixed with a precursor solution with an organic silicon source, on the one hand, it can play a supporting role and significantly enhance the stability and mechanical strength of the aerogel structure; on the other hand, the addition of highly hydrophobic graphene oxide aerogel can improve the hydrophobicity of the sol system and further improve the thermal insulation performance of the aerogel. DETAILED DESCRIPTION

[0024] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0025] The graphene oxide used in the present invention is prepared by the Hummers method, and the preparation steps are as follows:

[0026] Add 0.3 g of graphene to 2.4 mL of concentrated sulfuric acid, stir for 0.5 h, add 0.5 g of sodium nitrate, heat to 80 ° C, continue stirring for 5 h, add 12 mL of concentrated sulfuric acid, control the temperature to <5 ° C, slowly add 1.5 g of potassium permanganate, heat to 35 ° C, continue stirring for 2 h, then add 70 mL of deionized water and 2 mL of H2O2 (mass fraction of 30%), centrifuge, wash with 5% HCl and deionized water in turn to pH 7, and finally dry at 60 ° C for 65 h to obtain graphene oxide.

[0027] Example 1

[0028] This embodiment provides a method for preparing a high temperature resistant heat insulating aerogel, comprising the following steps:

[0029] Step 1: Add 0.2 g L-phenylalanine and 1 g graphene oxide to 100 mL deionized water, disperse by ultrasonic, adjust the pH to 10, stir at 90° C., cool and dialyze, and freeze-dry to obtain modified graphene oxide.

[0030] Step 2: 9 g of tetraethyl orthosilicate, 250 mL of anhydrous ethanol and 0.02 mL of nitric acid were mixed and stirred at room temperature to obtain a precursor solution; 0.3 g of modified graphene oxide was dissolved in 100 mL of anhydrous ethanol, and the mixture was mixed with the precursor solution after ultrasonic dispersion, and 0.1 mL of ammonia water (concentration of 0.5 mol / L) was added and stirred to obtain a sol;

[0031] Step 3, pressing the zirconia fiber into a fiber preform;

[0032] Step 4, immersing the fiber preform obtained in step 3 into the sol obtained in step 2, evacuating to -0.09 MPa, maintaining the pressure for 3 hours, and returning the pressure to normal pressure by introducing air to obtain a fiber and sol composite material;

[0033] Step 5: ageing, drying and sintering the fiber and sol composite material to obtain a high temperature resistant heat insulating aerogel.

[0034] Example 2

[0035] The only difference from Example 1 is that:

[0036] Step 1: Add 0.4 g L-phenylalanine and 1 g graphene oxide to 100 mL deionized water, disperse by ultrasonication, adjust the pH to 10.2, stir at 95° C., cool and dialyze, and freeze-dry to obtain modified graphene oxide.

[0037] The remaining materials and steps are the same as those in Example 1.

[0038] Example 3

[0039] The only difference from Example 1 is that:

[0040] Step 2, 8 g of methyl orthosilicate, 250 mL of anhydrous ethanol and 0.02 mL of hydrochloric acid were mixed, and stirred at room temperature to obtain a precursor solution; 0.4 g of modified graphene oxide was dissolved in 100 mL of anhydrous ethanol, and mixed with the precursor solution after ultrasonic dispersion, and 0.1 mL of ammonia water (concentration of 0.5 mol / L) was added and stirred continuously to obtain a sol;

[0041] The remaining materials and steps are the same as those in Example 1.

[0042] Example 4

[0043] The only difference from Example 1 is that:

[0044] Step 2: 10 g of methyl orthosilicate, 250 mL of anhydrous ethanol and 0.02 mL of sulfuric acid were mixed and stirred at room temperature to obtain a precursor solution; 0.5 g of modified graphene oxide was dissolved in 100 mL of anhydrous ethanol, and the mixture was mixed with the precursor solution after ultrasonic dispersion, and 0.1 mL of ammonia water (concentration of 0.5 mol / L) was added and stirred to obtain a sol;

[0045] The remaining materials and steps are the same as those in Example 1.

[0046] Example 5

[0047] The only difference from Example 1 is that:

[0048] Step 4, immersing the fiber preform obtained in step 3 into the sol obtained in step 2, evacuating to -0.1 MPa, maintaining the pressure for 2 hours, and returning the pressure to normal pressure by introducing air to obtain a fiber and sol composite material;

[0049] The remaining materials and steps are the same as those in Example 1.

[0050] Comparative Example 1

[0051] This comparative example provides a method for preparing a high temperature resistant heat insulating aerogel, comprising the following steps:

[0052] Step 1, 9 g of tetraethyl orthosilicate, 250 mL of anhydrous ethanol and 0.02 mL of nitric acid were mixed, and stirred at room temperature to obtain a precursor solution, and 0.1 mL of ammonia water (concentration of 0.5 mol / L) was added and continued to stir to obtain a sol;

[0053] Step 2, pressing the zirconia fiber into a fiber preform;

[0054] Step 3, immersing the fiber preform obtained in step 2 into the sol obtained in step 1, evacuating to -0.09 MPa, maintaining the pressure for 3 hours, and introducing air to restore the pressure to normal pressure to obtain a fiber and sol composite material;

[0055] Step 4: ageing, drying and sintering the fiber and sol composite material to obtain a high temperature resistant heat insulating aerogel.

[0056] Comparative Example 2

[0057] Compared with Example 1, 0.3 g of modified graphene oxide in step 2 is replaced by 0.25 g of modified graphene oxide; the remaining raw materials and steps are the same as those in Example 1.

[0058] Comparative Example 3

[0059] Compared with Example 4, 0.5 g of modified graphene oxide in step 2 is replaced by 0.55 g of modified graphene oxide; the remaining raw materials and steps are the same as those in Example 4.

[0060] The high temperature resistant heat insulating aerogels obtained in Examples 1-5 and Comparative Examples 1-3 were tested. Porosity test: The porosity (%) of the material was determined by the ratio of the sample block density to the density of the corresponding dense solid material using the mass-volume direct calculation method. The test was repeated 5 times and the average was taken as the final measurement result. The compressive strength of the aerogel was tested according to GB / T1449-2005 using Instron's ElectroPlus electronic dynamic static universal material testing machine. The results are shown in Table 1:

[0061] Table 1

[0062]

[0063] It can be seen from Table 1 that, compared with Comparative Examples 1-3, the high temperature resistant heat insulating aerogels obtained in Examples 1-5 all have high porosity, and also have lower density and thermal conductivity. No modified graphene oxide was added in Comparative Example 1, and the amount of graphene oxide added in Comparative Examples 2-3 exceeded the range specified in the present invention. It can be seen that whether modified magnesium hydroxide is used and its amount range will affect the porosity, thermal conductivity, density and compressive strength of the obtained aerogel.

[0064] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0065] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing a high temperature resistant heat insulating aerogel, characterized in that: The following steps are involved: Step 1, adding L-phenylalanine and graphene oxide into deionized water, ultrasonically dispersing, adjusting the pH to 10-10.2, stirring at 90-95° C., cooling and dialysis, and freeze-drying to obtain modified graphene oxide; Step 2, mixing a silicon source, anhydrous ethanol and an acid, and stirring at room temperature to obtain a precursor solution; dissolving the modified graphene oxide in anhydrous ethanol, mixing with the precursor solution after ultrasonic dispersion, adding a base and continuing stirring to obtain a sol; Step 3, pressing the fibers into a fiber preform; Step 4, immersing the fiber preform obtained in step 3 into the sol obtained in step 2, evacuating to -0.09 to -0.1 MPa, maintaining the pressure for 2 to 3 hours, and returning the pressure to normal pressure by introducing air to obtain a fiber and sol composite material; Step 5: ageing, drying and sintering the fiber and sol composite material to obtain a high temperature resistant heat insulating aerogel.

2. The method for preparing a high temperature resistant heat insulating aerogel according to claim 1, characterized in that: In step 1, the dosage ratio of L-phenylalanine, graphene oxide and deionized water is 0.2-0.4 g: 1 g: 100 mL.

3. The method for preparing a high temperature resistant heat insulating aerogel according to claim 1, characterized in that: In step 2, the usage ratio of silicon source, anhydrous ethanol, acid and base is 8-10 g: 250 mL: 0.02 mL: 0.1 mL; the usage ratio of modified graphene oxide and anhydrous ethanol is 0.3-0.5 g: 100 mL.

4. The method for preparing a high temperature resistant heat insulating aerogel according to claim 1, characterized in that: Graphene oxide was prepared by the Hummers method.

5. The method for preparing a high temperature resistant heat insulating aerogel according to claim 1, characterized in that: The silicon source is one of ethyl orthosilicate and methyl orthosilicate.

6. The method for preparing a high temperature resistant heat insulating aerogel according to claim 1, characterized in that: The acid is one of nitric acid, hydrochloric acid and sulfuric acid.

7. The method for preparing a high temperature resistant heat insulating aerogel according to claim 1, characterized in that: The base is aqueous ammonia.

8. The method for preparing a high temperature resistant heat insulating aerogel according to claim 1, characterized in that: The fiber is one of zirconia fiber, alumina fiber, quartz fiber and mullite fiber.

9. A high temperature resistant heat insulating aerogel, characterized in that: Prepared by the preparation method according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • Preparation method of oxidized graphene modified silicon dioxide aerogel fiber product adjustable in hydrophobic and hydrophilic property

    CN108793943A

  • Preparation method of high-temperature-resistant fiber-reinforced silicon dioxide aerogel thermal insulation composite material

    CN111302827A

  • Preparation method of graphene-organic silicon composite aerogel

    CN112138612A

  • Ultralow-oxygen-content three-dimensional nitrogen-doped graphene aerogel and preparation method thereof

    CN113387346A

  • Preparation method of high-temperature-resistant modified silicon oxide aerogel heat-insulation composite material

    CN115108809A