Preparation method of cordierite ceramic substrate

Through mechanical activation method and doping optimization formula, combined with MAS microcrystalline glass additive, the problems of low-temperature sintering densification and α-cordierite phase precipitation are solved, and the low-cost, low-temperature stability and high-frequency dielectric properties are achieved. Preparation of bluestone ceramic substrates, suitable for electronic packaging.

CN118930238APending Publication Date: 2024-11-12WUHAN UNIV OF TECH
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411076465.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The prior art is difficult to prepare dense cordierite ceramic substrates at low temperature sintering temperatures, and the precipitation of α-cordierite phases is difficult to affect its application in the field of electronic packaging.

Method used

The formulation and preparation process optimized by mechanical activation method and element doping are adopted to reduce the crystallinity and synthesis temperature of the raw materials through the combination of high-energy ball milling and ball milling media, and introduce MAS cordierite microcrystalline glass as a sintering additive to promote liquid phase sintering. and rearrangement of ceramic particles.

Benefits of technology

The densification of cordierite ceramics is achieved at lower temperatures, reducing production costs, and improving the low temperature stability and sintering driving force of α-cordierite ceramics, forming a cordierite ceramic substrate with low dielectric constant, suitable for Electronic packaging field.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930238A_ABST
    Figure CN118930238A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of a cordierite ceramic substrate, which comprises the following steps: S1, preparation and activation of a cordierite ceramic precursor: weighing magnesium oxide, aluminum oxide, silicon dioxide and a doping agent according to mass fraction, adding into a ball milling tank, mixing with deionized water, carrying out primary ball milling activation to obtain first slurry, and drying to obtain the cordierite ceramic precursor; the cordierite precursor powder is obtained; s2, adding the cordierite precursor powder obtained in the step S1, a sintering aid, an organic solvent and a dispersing agent into a ball-milling tank for secondary ball-milling and mixing, continuously adding a binder and a plasticizer into the ball-milling tank for tertiary ball-milling to obtain second slurry, forming the second slurry by using a tape casting process to obtain a green body, and sintering to obtain the cordierite ceramic material. The cordierite ceramic substrate is obtained. According to the method disclosed by the invention, densification of the cordierite ceramic substrate can be realized at a relatively low temperature, and the prepared cordierite ceramic substrate has a low dielectric constant.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of inorganic ceramic substrate manufacturing, and in particular to a method for preparing a cordierite ceramic substrate. Background Art

[0002] With the rapid development of high-frequency communication technology, 5G communication has a transmission speed of nearly 10 gigabits, a signal delay of less than 1 millisecond, a wide range of user access, and a greatly increased attenuation rate of several transmission signals in the sub-gigahertz and millisecond bands, making 5G communication more dependent on low dielectric constant materials.

[0003] High temperature stability of α-cordierite (1100-1450℃) in cordierite ceramics (2MgO.2Al2O3.5SiO2, MAS) has low dielectric constant, low dielectric loss, low thermal expansion coefficient (≤2×10 -6 K -1 ), good thermal stability and mechanical strength, and is widely used in refractory ceramic materials, honeycomb ceramic catalyst carriers, electronic devices and microelectronic packaging. In actual application, Mg-Al-Si cordierite glass-ceramics are often used in the field of electronic packaging (melting temperature up to 1600°C, high production cost, and difficult process), while cordierite ceramics are often used as kiln tools and are less used in the field of ceramic substrates. This is because cordierite ceramics have high liquid phase viscosity, low sintering driving force, and a narrow sintering temperature range, generally around 1400-1440°C. Sintering at lower temperatures usually results in porous cordierite ceramics, and dense cordierite ceramics cannot be obtained. At higher sintering temperatures, cordierite ceramics tend to form a large amount of glass phase, so it is more difficult to prepare dense cordierite ceramics.

[0004] How to achieve the densification of cordierite ceramics and the precipitation of α-cordierite phase at a low-temperature sintering temperature (1100°C) is the key to the application of cordierite ceramics in the field of packaging technology. Summary of the invention

[0005] In order to solve the problems existing in the background technology, the present invention provides a method for preparing a cordierite ceramic substrate, which can realize the densification of the cordierite ceramic substrate at a relatively low temperature, and the prepared cordierite ceramic substrate has a low dielectric constant.

[0006] The technical solution of the present invention to solve the above technical problems is as follows:

[0007] A method for preparing a cordierite ceramic substrate comprises the following steps:

[0008] S1. Configuration and activation of cordierite ceramic precursor: magnesium oxide, aluminum oxide, silicon dioxide and dopant are weighed by mass fraction, added to a ball mill and mixed with deionized water, and a ball milling activation is performed to obtain a first slurry, which is dried to obtain the cordierite precursor powder;

[0009] S2. Add the cordierite precursor powder, sintering aid, organic solvent and dispersant obtained in step S1 into a ball mill for secondary ball milling and mixing, continue to add a binder and a plasticizer into the ball mill for a third ball milling to obtain a second slurry, use a tape casting process to mold the second slurry into a green body, and sinter to obtain the cordierite ceramic substrate.

[0010] According to the above scheme, the dopant in step S1 is one or more of Li2CO3, K2CO3, and Na2CO3.

[0011] According to the above scheme, the weight percentages of the raw material components in step S1 are as follows: 5-25wt% magnesium oxide, 18-32wt% aluminum oxide, 47-58wt% silicon dioxide, and 1-3wt% dopant. The sum of the weight percentages of the above components is 100%.

[0012] According to the above scheme, a high-energy ball mill is used in step S1, the rotation speed of the ball mill is 200-400 r / min, and the ball milling time is 24-48 h. During the ball milling process, the materials are fully mixed, broken, combined, and activated. The particle size of the first slurry after ball milling is tested, and the particle size D50 of the first slurry is controlled at 0.3-0.8 μm. If it does not meet the particle size requirements, continue ball milling.

[0013] According to the above scheme, after drying, pass through an 80-mesh sieve.

[0014] The drying temperature is 60-80°C.

[0015] Since the ball milling process will cause wear of the ball milling medium, in order to avoid the introduction of impurities, preferably, the ball milling medium in the high-energy ball mill in step S1 is alumina balls, and the weight ratio of the raw material, deionized water and alumina balls is 1:1~3:20~40. Since alumina will be introduced during the ball milling process, the weighed amount of alumina in the raw material is 2~4wt% lower than the calculated value.

[0016] According to the above scheme, a common horizontal ball mill can be used for ball milling in step S2.

[0017] According to the above scheme, the sintering aid in step S2 is MAS (MgO-Al2O3-SiO2) cordierite glass-ceramics, and the added amount is 1 to 3 wt% of the cordierite precursor powder.

[0018] According to the above scheme, the organic solvent in step S2 is a mixed solvent of ethanol and acetone, the dispersant is triethyl phosphate, the binder is polyvinyl butyral, and the plasticizer is dibutyl phthalate.

[0019] According to the above scheme, in the mixed solvent composed of ethanol and acetone, the mass fraction of ethanol is 60% to 70%.

[0020] According to the above scheme, the added amounts of the dispersant, the binder and the plasticizer are 2-4wt%, 3-5wt% and 2-4wt% of the cordierite precursor powder respectively.

[0021] According to the above scheme, in step S2, the green body is debinded according to a temperature increase system of 2°C / min, and sintered at 1100-1200°C for 2-4h.

[0022] According to the above scheme, the ball milling medium for the secondary ball milling in step S2 is alumina balls, the amount of organic solvent added is 1 to 3 times the mass of cordierite precursor powder, sintering aid, and dispersant, and the amount of alumina balls added is 3 to 5 times the mass of cordierite precursor powder, sintering aid, and dispersant.

[0023] The beneficial effects of the present invention are:

[0024] The invention uses mechanical activation method and element doping to optimize the formula and preparation process of cordierite. The mechanical activation method breaks raw materials such as MgO, Al2O3, SiO2, etc., so that each crystal has defects, dislocations and lattice distortions, reduces the crystallinity of the raw materials, increases the specific surface area, and enhances the reaction activity between the raw materials. The introduced dopant with a smaller ion radius enters the gap of the cordierite ring structure and partially replaces Mg. 2+ , causing its lattice distortion, reducing the synthesis temperature of α-cordierite ceramics, enabling α-cordierite to be synthesized at a lower temperature, effectively improving the low-temperature stability of α-cordierite and reducing the production cost; finally, during the sintering process, by introducing MAS cordierite glass-ceramics of the same component, the glass phase in the sintering process is increased to form liquid phase sintering (the flow mass transfer rate is significantly higher than the diffusion mass transfer, and during the liquid phase sintering process, the liquid phase flows into the particle gaps under the action of capillary force, which can accelerate the rearrangement of ceramic particles), thereby accelerating the diffusion mass transfer process between ceramic powders, increasing the driving force for the sintering of cordierite ceramics, and promoting the densification of cordierite ceramics under low-temperature sintering. On the other hand, using cordierite glass-ceramics as a sintering aid instead of traditional low-melting-point oxide sintering aids also avoids the introduction of impurities due to the addition of sintering aids, thereby reducing the performance of the cordierite ceramic substrate. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1This is the XRD diffraction pattern of the cordierite ceramic substrate prepared in Example 1 of the present invention;

[0026] Figure 2 This is a SEM photo of the cordierite ceramic substrate prepared in Example 1 of the present invention;

[0027] Figure 3 The dielectric properties of the cordierite ceramic substrate prepared in Example 1 of the present invention at different frequencies. DETAILED DESCRIPTION

[0028] The principles and features of the present invention are described below in conjunction with the accompanying drawings and specific embodiments. The examples given are only used to explain the present invention and are not used to limit the scope of the present invention.

[0029] It should be noted that in the description of the embodiments of the present application, the description of the term "some specific embodiments" means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same implementation or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0030] The present invention provides a method for preparing a cordierite ceramic substrate, comprising the following steps:

[0031] S1. Configuration and activation of cordierite ceramic precursor: magnesium oxide, aluminum oxide, silicon dioxide and dopant are weighed by mass fraction, added to a ball mill and mixed with deionized water, and a ball milling activation is performed to obtain a first slurry, which is dried to obtain the cordierite precursor powder;

[0032] S2. Add the cordierite precursor powder, sintering aid, organic solvent and dispersant obtained in step S1 into a ball mill for secondary ball milling and mixing, continue to add a binder and a plasticizer into the ball mill for a third ball milling to obtain a second slurry, use a tape casting process to mold the second slurry into a green body, and sinter to obtain the cordierite ceramic substrate.

[0033] In some specific embodiments, the dopant in step S1 is one or more of Li2CO3, K2CO3, and Na2CO3.

[0034] In some specific embodiments, the weight percentages of the raw material components in step S1 are as follows: 5-25wt% magnesium oxide, 18-32wt% aluminum oxide, 47-58wt% silicon dioxide, and 1-3wt% dopant, and the sum of the weight percentages of the above components is 100%.

[0035] In some specific embodiments, a high-energy ball mill is used in step S1, the rotation speed of the ball mill is 200-400 r / min, the ball milling time is 24-48 h, and the particle size D50 of the first slurry is controlled at 0.3-0.8 μm.

[0036] In some specific embodiments, the ball milling medium in the high energy ball mill in step S1 is alumina balls, the weight ratio of the raw material, deionized water and alumina balls is 1:1-3:20-40, and the weighed amount of alumina in the raw material is 2-4wt% lower than the calculated value.

[0037] In some specific embodiments, the sintering aid in step S2 is MAS (MgO-Al2O3-SiO2) cordierite glass-ceramics, and the added amount is 1 to 3 wt% of the cordierite precursor powder.

[0038] In some specific embodiments, the MAS cordierite glass-ceramic is Corning 9606 glass.

[0039] In some specific embodiments, the organic solvent in step S2 is a mixed solvent of ethanol and acetone, the dispersant is triethyl phosphate, the binder is polyvinyl butyral, and the plasticizer is dibutyl phthalate.

[0040] In some specific embodiments, ethanol accounts for 60% to 70% of the mixed solvent by mass.

[0041] In some specific embodiments, the added amounts of the dispersant, the binder and the plasticizer are 2-4 wt%, 3-5 wt% and 2-4 wt% of the cordierite precursor powder, respectively.

[0042] In some specific embodiments, in step S2, the green body is debinded according to a temperature increase system of 2° C. / min, and sintered at 1100-1200° C. for 2-4 hours.

[0043] In some specific embodiments, the ball milling medium for the secondary ball milling in step S2 is alumina balls, the amount of organic solvent added is 1 to 3 times the mass of cordierite precursor powder, sintering aid, and dispersant, and the amount of alumina balls added is 3 to 5 times the mass of cordierite precursor powder, sintering aid, and dispersant.

[0044] On the basis of the above-mentioned embodiments, the present invention provides the following specific examples to further illustrate the present invention. It should be understood that these examples are only used to illustrate the present invention and are not used to limit the scope of the present invention. The experimental methods without specifying specific conditions in the following examples are usually based on the conditions recommended by the manufacturer. Unless otherwise stated, percentages and parts are calculated by mass.

[0045] Among them, MAS (MgO-Al2O3-SiO2) cordierite glass-ceramics uses Corning 9606 glass.

[0046] Example 1

[0047] This embodiment provides a method for preparing a cordierite ceramic substrate, comprising the following steps:

[0048] (1) Ingredients: 20 wt% magnesium oxide, 20 wt% aluminum oxide, 50 wt% silicon dioxide, and 2 wt% Li2CO3 were weighed using a 1 / 1000 electronic balance;

[0049] (2) Primary ball milling: the weighed raw materials were added into the ball milling tank of a high-energy planetary ball mill and ball milled for 24 hours, with the ratio of water: material: ball milling medium (Al2O3 balls) being 1:1:20 and the ball mill speed being 400 r / min;

[0050] (3) Particle size testing, drying and sieving: The mixed material that meets the particle size requirements (particle size D50 is 0.3-0.8 μm) is fully dried in an oven at 80°C and passed through an 80-mesh sieve;

[0051] (4) Secondary ball milling: Add cordierite precursor powder (100 g) that meets the particle size requirements, 9606 glass (1 g), ethanol / acetone (110 g, mass ratio 7:3), and triethyl phosphate (3 g) into a ball mill and mill for 24 hours;

[0052] (5) Third ball milling: polyvinyl butyral (PVB) (10 g) and dibutyl phthalate (3 g) were added to the ball mill and ball milled for 24 hours to obtain a second slurry;

[0053] (6) molding: molding the second slurry using a tape casting process to obtain a green body;

[0054] (7) Sintering: The green body is debinded according to a heating system of 2°C / min and sintered at 1100°C for 2 hours to finally obtain the desired cordierite ceramic substrate.

[0055] Example 2

[0056] This embodiment provides a method for preparing a cordierite ceramic substrate, comprising the following steps:

[0057] (1) Ingredients: 15 wt% magnesium oxide, 25 wt% aluminum oxide, 55 wt% silicon dioxide, and 1 wt% Na2CO3 were weighed using a 1 / 1000 electronic balance;

[0058] (2) Primary ball milling: the weighed raw materials were added into the ball milling tank of a high-energy planetary ball mill and ball milled for 24 hours, with a water: material: ball milling medium (Al2O3 ball) ratio of 1:1:30 and a ball mill speed of 400 r / min;

[0059] (3) Particle size testing, drying and sieving: The mixed material that meets the particle size requirements (particle size D50 is 0.3-0.8 μm) is fully dried in an oven at 80°C and passed through an 80-mesh sieve;

[0060] (4) Secondary ball milling: Add cordierite precursor powder (100 g) that meets the particle size requirements, 9606 glass (2 g), ethanol / acetone (110 g, mass ratio 7:3), and triethyl phosphate (3 g) into a ball mill and mill for 24 hours;

[0061] (5) Third ball milling: polyvinyl butyral (PVB) (10 g) and dibutyl phthalate (3 g) were added to the ball mill and ball milled for 24 hours to obtain a second slurry;

[0062] (6) molding: molding the second slurry using a tape casting process to obtain a green body;

[0063] (7) Sintering: The green body was debinded according to a heating system of 2°C / min and sintered at 1150°C for 2.5 h to finally obtain the desired cordierite ceramic substrate.

[0064] Example 3

[0065] This embodiment provides a method for preparing a cordierite ceramic substrate, the method comprising the following steps:

[0066] (1) Ingredients: 23 wt% magnesium oxide, 30 wt% aluminum oxide, 47 wt% silicon dioxide, and 3 wt% K2CO3 were weighed using a 1 / 1000 electronic balance;

[0067] (2) Primary ball milling: the weighed raw materials were added into the ball milling tank of a high-energy planetary ball mill and ball milled for 24 hours, with the ratio of water: material: ball milling medium (Al2O3 balls) being 1:1:40 and the ball mill speed being 400 r / min;

[0068] (3) Particle size testing, drying and sieving: The mixed material that meets the particle size requirements (particle size D50 is 0.3-0.8 μm) is fully dried in an oven at 80°C and passed through an 80-mesh sieve;

[0069] (4) Secondary ball milling: Add cordierite precursor powder (100 g) that meets the particle size requirements, 9606 glass (3 g), ethanol / acetone (110 g, mass ratio 7:3), and triethyl phosphate (3 g) into a ball mill and mill for 24 hours;

[0070] (5) Third ball milling: polyvinyl butyral (PVB) (10 g) and dibutyl phthalate (3 g) were added to the ball mill and ball milled for 24 hours to obtain a second slurry;

[0071] (6) Molding: Using a tape casting process to mold the second slurry to obtain a green body

[0072] (7) Sintering: The green body is debinded according to a heating system of 2°C / min and sintered at 1200°C for 3 hours to finally obtain the desired cordierite ceramic substrate.

[0073] Comparative Example 1

[0074] The only difference between Comparative Example 1 and Example 1 is that the dopant Li2CO3 is not added.

[0075] Comparative Example 2

[0076] The difference between Comparative Example 2 and Example 1 is that during the first ball milling process, water: material: ball milling medium (Al2O3 balls) = 1:1:3, and the ball mill speed is 200r / min.

[0077] Comparative Example 3

[0078] The only difference between Comparative Example 3 and Example 1 is that no sintering aid MAS cordierite glass-ceramics is added.

[0079] The cordierite ceramic substrates prepared in Example 1 and the comparative example were characterized and tested for performance, and the results were as follows:

[0080] Figure 1 The XRD diffraction pattern of the cordierite ceramic substrate prepared in Example 1 shows that the phase structure of the obtained sample is α-cordierite phase, and no impurities such as MgO, Al2O3, SiO2, and Li2CO3 are detected, indicating that the raw materials react fully during the synthesis process. It also proves that the precipitation of α-cordierite phase can be achieved at 1100°C using this synthesis method.

[0081] Figure 2 This is a scanning electron microscope (SEM) photograph of the cordierite ceramic substrate prepared in Example 1. It can be seen from the figure that the cordierite ceramic particles are tightly combined and have fewer pores, indicating that the cordierite ceramic prepared by this method has a higher density. In addition, the grain boundaries of the cordierite ceramic are relatively blurred, indicating that the introduced MAS cordierite glass-ceramics form a large amount of glass phase, which is enriched in the gaps between the grains and promotes the densification of the cordierite ceramic.

[0082] The dielectric properties of the cordierite ceramic substrate prepared in Example 1 at different frequencies were measured. The results are as follows: Figure 3 As shown in Figure 2, its relative dielectric constant is between 5.0 and 5.2, which is much lower than the cordierite ceramics (relative dielectric constant = 6) and Al2O3 ceramics (relative dielectric constant = 9.8) prepared by traditional methods. The dielectric loss is ≤10 at high frequencies. -4, meeting application requirements, the cordierite ceramic substrate prepared by this method is expected to replace the alumina substrate in the packaging field.

[0083] The density and porosity of the cordierite ceramic substrates prepared in Examples 1-3 and Comparative Examples 1-3 were measured respectively, and the results are shown in Table 1 below.

[0084] Table 1 Density and porosity of cordierite ceramic substrates prepared in Examples 1-3 and Comparative Examples 1-3

[0085]

[0086] As can be seen from the above table, the cordierite ceramics treated with mechanical activation, doping modification and addition of sintering aids all have a high density; Comparative Example 1 does not add a modifier, Comparative Example 2 only uses ordinary ball milling to simply disperse the raw materials, and Comparative Example 3 does not add MAS cordierite microcrystalline glass as a sintering aid. The above three comparative examples cannot achieve the densification of cordierite ceramics, indicating that lattice distortion, powder surface defects and the liquid phase formed by the sintering aid are all conducive to the sintering of cordierite ceramics. Lattice distortion and powder surface defects are conducive to improving the sintering activity of the powder, and the liquid phase formed by the sintering aid can accelerate the mass transfer process and promote the rearrangement of ceramic particles. In addition, it can be seen from Table 1 that the three improvement measures to promote ceramic sintering are indispensable.

[0087] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a cordierite ceramic substrate, characterized in that: The steps include: S1. Configuration and activation of cordierite ceramic precursor: magnesium oxide, aluminum oxide, silicon dioxide and dopant are weighed according to mass fraction, added to a ball mill and mixed with deionized water, and a first slurry is obtained by ball milling activation, and dried to obtain a cordierite precursor powder; S2. Add the cordierite precursor powder, sintering aid, organic solvent and dispersant obtained in step S1 into a ball mill for secondary ball milling and mixing, continue to add a binder and a plasticizer into the ball mill for a third ball milling to obtain a second slurry, use a tape casting process to mold the second slurry into a green body, and sinter to obtain the cordierite ceramic substrate.

2. The method for preparing a cordierite ceramic substrate according to claim 1, characterized in that: The dopant in step S1 is one or more of Li2CO3, K2CO3, and Na2CO3.

3. The method for preparing a cordierite ceramic substrate according to claim 1, characterized in that: The weight percentages of the raw material components in step S1 are as follows: 5-25wt% magnesium oxide, 18-32wt% aluminum oxide, 47-58wt% silicon dioxide, and 1-3wt% dopant. The sum of the weight percentages of the above components is 100%.

4. The method for preparing a cordierite ceramic substrate according to claim 1, characterized in that: In step S1, a high-energy ball mill is used, the rotation speed of the ball mill is 200-400 r / min, and the ball milling time is 24-48 hours, so that the particle size D50 of the first slurry is controlled at 0.3-0.8 μm.

5. The method for preparing a cordierite ceramic substrate according to claim 4, characterized in that: In step S1, the ball milling medium in the high energy ball mill is alumina balls, the weight ratio of the raw material, deionized water and alumina balls is 1:1-3:20-40, and the weighed amount of alumina in the raw material is 2-4wt% lower than the calculated value.

6. The method for preparing a cordierite ceramic substrate according to claim 1, characterized in that: The sintering aid in step S2 is MAS (MgO-Al2O3-SiO2) cordierite glass-ceramics, and the added amount is 1 to 3 wt% of the cordierite precursor powder.

7. The method for preparing a cordierite ceramic substrate according to claim 1, characterized in that: In step S2, the organic solvent is a mixed solvent of ethanol and acetone, the dispersant is triethyl phosphate, the binder is polyvinyl butyral, and the plasticizer is dibutyl phthalate.

8. The method for preparing a cordierite ceramic substrate according to claim 1, characterized in that: The added amounts of the dispersant, the binder and the plasticizer are 2-4wt%, 3-5wt% and 2-4wt% of the cordierite precursor powder respectively.

9. The method for preparing a cordierite ceramic substrate according to claim 1, characterized in that: The sintering time in step S2 is 2 to 4 hours, and the sintering temperature is 1100 to 1200°C.

10. The method for preparing a cordierite ceramic substrate according to claim 1, characterized in that: The ball milling medium for the secondary ball milling in step S2 is alumina balls, the amount of organic solvent added is 1 to 3 times the mass of cordierite precursor powder, sintering aid and dispersant, and the amount of alumina balls added is 3 to 5 times the mass of cordierite precursor powder, sintering aid and dispersant.

Citation Information

Patent Citations

  • Bonding method based lamination process of cordierite ceramic blank piece

    CN103342550A

  • Cordierite ceramic material with ultralow coefficient of thermal expansion and preparation method thereof

    CN103803957A

  • Method for preparing Ta2AlC monolithic ceramics by mechanical activating and hot-pressing

    CN104909757A

  • Method for preparing cordierite ceramic through reactive sintering

    CN117263665A

  • Preparation method of toughened ceramic sheet for microcrystalline glass

    CN117736005A