Manganese zinc ferrite material and preparation method thereof
By adjusting the proportion of the main and auxiliary components of manganese-zeb ferrite materials, adding cobalt elements, and controlling the sintering process, the problems of low magnetic permeability and low Curie temperature of manganese-zeb ferrite materials are solved, and high magnetic conductivity is achieved Manganese zinc ferrite materials with high Curie temperature are suitable for electronic components in high temperature environments.
Patent Information
- Application Number
- CN202310514637.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-09
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2043-05-09
AI Technical Summary
The existing manganese-zeb ferrite materials have problems with low magnetic permeability and low Curie temperature, making it difficult to maintain stable operation in high temperature environments.
By adjusting the ratio of main and auxiliary components, adding cobalt elements, and strictly controlling the sintering process parameters, manganese-zeb ferrite materials with high permeability, high Curie temperature, wide temperature, broad frequency, and low temperature coefficient are prepared.
It achieves high permeability (15000-16000) and high Curie temperature (≥136℃) in the temperature range of 0-60℃, and reduces the temperature coefficient, meeting the stable working needs of electronic components in high temperature environments.
Smart Images

Figure BDA0004218630500000121 
Figure BDA0004218630500000131
Abstract
Description
Technical Field
[0001] The invention relates to the field of ferrite, and in particular to a manganese-zinc ferrite material and a preparation method thereof. Background Art
[0002] At present, high permeability manganese-zinc ferrite is widely used in the fields of electronic signal transmission, anti-electromagnetic interference technology, environmental protection and energy saving. With the rapid development of electronic information industries such as communications, computers, and networks, and technological advances such as high-frequency and high-speed integrated circuits and micro-electromechanical systems, the total power density of electronic components has increased, and the demand for electronic components has become more miniaturized and integrated. However, as the size of electronic components becomes smaller, the heat flux density will increase sharply, and the operating temperature around the electronic components will increase significantly. It is a huge test for electronic components to work stably in a high temperature environment. Therefore, the development of high Curie temperature materials is required. With the development of electronic devices, the demand for materials is becoming more and more multifunctional: manganese-zinc ferrite with high permeability, wide temperature, wide frequency, low temperature coefficient and high Curie temperature.
[0003] For example, CN104628371A discloses a manganese-zinc ferrite with high initial magnetic permeability and high Curie temperature, the main components of which are 51-54 mol% iron oxide, 20-26 mol% zinc oxide, and the rest is manganese oxide. The auxiliary agents are 50-300 ppm calcium oxide, 10-800 ppm bismuth oxide, 20-1500 ppm titanium dioxide, and 10-500 ppm titanium oxide. Within the composition range of this solution, the magnetic permeability Curie temperature is greater than 135°C, and the magnetic permeability is much lower than 15000 (10KHz, 0.25mT). It can be seen that it is difficult to achieve consistency with an initial magnetic permeability of more than 15000 and a Curie temperature greater than or equal to 135°C.
[0004] For example, CN103833346A discloses a broadband manganese-zinc ferrite material and its preparation method, wherein the iron oxide is in the range of 52.0-53.0 mol%, the zinc oxide is in the range of 20.0-22.5 mol%, and the rest is manganese oxide, Bs (25°C) 462 mT, although the Curie temperature reaches 136°C. However, the initial magnetic permeability μi (25°C, 10KHz, 200KHZ) is less than 14000. The initial magnetic permeability is relatively low.
[0005] It can be seen that the manganese-zinc ferrite material in the prior art still has the problems of low magnetic permeability and low Curie temperature. Summary of the invention
[0006] In view of the problems existing in the prior art, the object of the present invention is to provide a manganese-zinc ferrite material and a preparation method thereof, so as to solve the problems of low magnetic permeability and low Curie temperature still existing in the manganese-zinc ferrite material.
[0007] To achieve this object, the present invention adopts the following technical solutions:
[0008] In a first aspect, the present invention provides a manganese-zinc ferrite material, the manganese-zinc ferrite material comprising a main component and an auxiliary component;
[0009] The main components include ZnO 19.6-21.48 mol%, MnO 26.02-29.52 mol%, and the balance is Fe2O3 in terms of molar percentage;
[0010] The auxiliary components include: CaCO3 100-2000ppm, Bi2O3 200-2000ppm, MoO 100-2000ppm, CoO 100-1500ppm, based on the main component.
[0011] The manganese-zinc ferrite material provided by the present invention can obtain a manganese-zinc ferrite material with high magnetic permeability, high Curie temperature (≥135°C), wide temperature, wide frequency, and low temperature coefficient characteristics through the main formula range and the auxiliary component range. Among them, the cobalt element is added as an auxiliary agent, the content of Fe in the main formula is reduced, and the proportion of iron, manganese, and zinc is strictly controlled to ensure high magnetic permeability. Furthermore, the cobalt element and the iron element after sintering in the main component are added in a reasonable ratio, and the two peak positions are adjusted to flatten the temperature curve, so that μi (25°C-60°C) reaches the range of 15000-16000 and has a lower temperature coefficient.
[0012] In the present invention, the molar percentage of ZnO in the main component of the manganese-zinc ferrite material is 19.6-21.48 mol%, for example, it can be 19.6 mol%, 19.7 mol%, 19.8 mol%, 19.9 mol%, 20 mol%, 20.1 mol%, 20.2 mol%, 20.3 mol%, 20.4 mol%, 20.5 mol%, 20.6 mol%, 20.7 mol%, 20.8 mol%, 20.9 mol%, 21 mol%, 21.1 mol%, 21.2 mol%, 21.3 mol%, 21.4 mol% or 21.48 mol%, etc., but is not limited to the listed values, and other values not listed within the range are equally applicable.
[0013] In the present invention, the molar percentage of MnO in the main component of the manganese-zinc ferrite material is 26.02-29.52 mol%, for example, it can be 26.02 mol%, 26.2 mol%, 26.4 mol%, 26.6 mol%, 26.8 mol%, 27 mol%, 27.2 mol%, 27.4 mol%, 27.6 mol%, 27.8 mol%, 28 mol%, 28.2 mol%, 28.4 mol%, 28.6 mol%, 28.8 mol%, 29 mol%, 29.2 mol%, 29.4 mol% or 29.52 mol%, but is not limited to the listed values, and other values not listed within the range are equally applicable.
[0014] In the present invention, based on the main component, the content of CaCO3 in the auxiliary component is 100-2000ppm, for example, it can be 100ppm, 200ppm, 300ppm, 400ppm, 500ppm, 600ppm, 700ppm, 800ppm, 900ppm, 1000ppm, 1100ppm, 1200ppm, 1300ppm, 1400ppm, 1500ppm, 1600ppm, 1700ppm, 1800ppm, 1900ppm or 2000ppm, but is not limited to the listed values, and other unlisted values within the range are equally applicable.
[0015] In the present invention, based on the main component, the content of Bi2O3 in the auxiliary component is 200-2000ppm, for example, it can be 200ppm, 300ppm, 400ppm, 500ppm, 600ppm, 700ppm, 800ppm, 900ppm, 1000ppm, 1100ppm, 1200ppm, 1300ppm, 1400ppm, 1500ppm, 1600ppm, 1700ppm, 1800ppm, 1900ppm or 2000ppm, but is not limited to the listed values, and other values not listed within the range are also applicable.
[0016] In the present invention, based on the main component, the content of MoO in the auxiliary component is 100-2000ppm, for example, it can be 100ppm, 200ppm, 300ppm, 400ppm, 500ppm, 600ppm, 700ppm, 800ppm, 900ppm, 1000ppm, 1100ppm, 1200ppm, 1300ppm, 1400ppm, 1500ppm, 1600ppm, 1700ppm, 1800ppm, 1900ppm or 2000ppm, but is not limited to the listed values, and other values not listed within the range are also applicable.
[0017] In the present invention, based on the main component, the content of CoO in the auxiliary component is 100-1500ppm, for example, it can be 100ppm, 200ppm, 300ppm, 400ppm, 500ppm, 600ppm, 700ppm, 800ppm, 900ppm, 1000ppm, 1100ppm, 1200ppm, 1300ppm, 1400ppm or 1500ppm, but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0018] As a preferred technical solution of the present invention, the manganese-zinc ferrite material includes a main component and an auxiliary component;
[0019] The main components include ZnO 20-21.2mol%, MnO 27-28mol%, and the balance is Fe2O3 in terms of molar percentage;
[0020] The auxiliary components include: CaCO3 200-400ppm, Bi2O3 450-600ppm, MoO200-800ppm, CoO1000-1500ppm, based on the main component.
[0021] In a second aspect, the present invention provides a method for preparing the manganese-zinc ferrite material as described in the first aspect, the preparation method comprising:
[0022] Prepare main ingredients and auxiliary ingredients according to the formula;
[0023] The main component material is ball-milled, dried and pre-calcined in sequence, then mixed with the auxiliary component material, sand-milled, and dried to obtain a ferrite mixture;
[0024] The obtained ferrite mixture is heat-treated in sequence, and then mixed with a binder and granulated to obtain ferrite particles, which are sintered in a mixed atmosphere and then cooled to obtain a manganese-zinc ferrite material.
[0025] In the present invention, cooling after sintering is performed under a balanced oxygen partial pressure.
[0026] As a preferred technical solution of the present invention, the ball milling method is wet ball milling.
[0027] Preferably, the mass ratio of material to grinding balls in the ball mill is 1:(7-8), for example, it can be 1:7, 1:7.1, 1:7.2, 1:7.3, 1:7.4, 1:7.5, 1:7.6, 1:7.7, 1:7.8, 1:7.9 or 1:8, but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0028] Preferably, the ball milling time is 30-50 min, for example, it can be 30 min, 31 min, 32 min, 33 min, 34 min, 35 min, 36 min, 37 min, 38 min, 39 min, 40 min, 41 min, 42 min, 43 min, 44 min, 45 min, 46 min, 47 min, 48 min, 49 min or 50 min, but is not limited to the listed values, and other values not listed in the range are also applicable.
[0029] Preferably, the pre-firing temperature is 700-800°C, for example, it can be 700°C, 710°C, 720°C, 730°C, 740°C, 750°C, 760°C, 770°C, 780°C, 790°C or 800°C, but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0030] Preferably, the pre-burning time is 2-3h, for example, it can be 2h, 2.1h, 2.2h, 2.3h, 2.4h, 2.5h, 2.6h, 2.7h, 2.8h, 2.9h or 3h, but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0031] In the present invention, pre-sintering makes the auxiliary agent more evenly distributed, thereby achieving high initial magnetic permeability, wide temperature range and low temperature coefficient of the Mn-Zn ferrite material.
[0032] As a preferred technical solution of the present invention, the sanding method is wet sanding.
[0033] Preferably, the sanding time is 70-90 min, for example, it can be 70 min, 71 min, 72 min, 73 min, 74 min, 75 min, 76 min, 77 min, 78 min, 79 min, 80 min, 81 min, 82 min, 83 min, 84 min, 85 min, 86 min, 87 min, 88 min, 89 min or 90 min, but is not limited to the listed values, and other values not listed in the range are also applicable.
[0034] As a preferred technical solution of the present invention, the temperature of the heat treatment is 700-850°C, for example, it can be 700°C, 710°C, 720°C, 730°C, 740°C, 750°C, 760°C, 770°C, 780°C, 790°C, 800°C, 810°C, 820°C, 830°C, 840°C or 850°C, etc., but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0035] Preferably, the heat treatment time is 3-3.5 h, for example, 3 h, 3.1 h, 3.2 h, 3.3 h, 3.4 h or 3.5 h, etc., but is not limited to the listed values, and other values not listed within the range are also applicable.
[0036] As a preferred technical solution of the present invention, the adhesive includes polyvinyl alcohol.
[0037] Preferably, the amount of the adhesive added is 8-10% of the mass of the ferrite mixture, for example, it can be 8%, 8.1%, 8.2%, 8.3%, 8.4%, 8.5%, 8.6%, 8.7%, 8.8%, 8.9%, 9%, 9.1%, 9.2%, 9.3%, 9.4%, 9.5%, 9.6%, 9.7%, 9.8%, 9.9% or 10%, etc., but is not limited to the listed values, and other values not listed in this range are also applicable.
[0038] As a preferred technical solution of the present invention, the mixed atmosphere includes protective gas and oxygen, and the volume percentage of oxygen is 3-21%, for example, it can be 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20% or 21%, etc., but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0039] Preferably, the protective gas includes one or a combination of at least two of nitrogen, helium, neon or argon.
[0040] As a preferred technical solution of the present invention, the sintering includes a first sintering;
[0041] Preferably, the first sintering is sintering at 1280-1350° C. for 4-10 h in a mixed atmosphere with an oxygen content of 3-8% by volume.
[0042] In the present invention, the volume percentage of oxygen in the mixed atmosphere in the first sintering is 3-8%, for example, it can be 3%, 3.2%, 3.4%, 3.6%, 3.8%, 4%, 4.2%, 4.4%, 4.6%, 4.8%, 5%, 5.2%, 5.4%, 5.6%, 5.8%, 6%, 6.2%, 6.4%, 6.6%, 6.8%, 7%, 7.2%, 7.4%, 7.6%, 7.8% or 8%, etc., but is not limited to the listed values, and other values not listed in the range are also applicable.
[0043] In the present invention, the temperature of the first sintering is 1280-1350°C, for example, it can be 1280°C, 1285°C, 1290°C, 1295°C, 1300°C, 1305°C, 1310°C, 1315°C, 1320°C, 1325°C, 1330°C, 1335°C, 1340°C, 1345°C or 1350°C, but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0044] In the present invention, the first sintering time is 4-10h, for example, it can be 4h, 4.5h, 5h, 5.5h, 6h, 6.5h, 7h, 7.5h, 8h, 8.5h, 9h, 9.5h or 10h, but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0045] Preferably, the first sintering further includes a second sintering and a third sintering performed in sequence.
[0046] In the present invention, the use of specific multi-stage sintering is beneficial to further improve the performance of the obtained manganese-zinc ferrite material.
[0047] In the present invention, when the sintering is multi-stage sintering, the time of the first sintering can be 4-8 hours, for example, it can be 4h, 4.5h, 5h, 5.5h, 6h, 6.5h, 7h, 7.5h or 8h, but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0048] Preferably, the second sintering is sintering at 600-700° C. for 1-3 h in a mixed atmosphere with an oxygen content of 19-21% by volume.
[0049] In the present invention, the volume percentage of oxygen in the mixed atmosphere of the second sintering is 19-21%, for example, it can be 19%, 19.1%, 19.2%, 19.3%, 19.4%, 19.5%, 19.6%, 19.7%, 19.8%, 19.9%, 20%, 20.1%, 20.2%, 20.3%, 20.4%, 20.5%, 20.6%, 20.7%, 20.8%, 20.9% or 21%, etc., but is not limited to the listed values, and other values not listed in the range are also applicable.
[0050] In the present invention, the temperature of the second sintering is 600°C-700°C, for example, it can be 600°C, 610°C, 620°C, 630°C, 640°C, 650°C, 660°C, 670°C, 680°C, 690°C or 700°C, but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0051] In the present invention, the time of the second sintering is 1-3h, for example, it can be 1h, 1.1h, 1.2h, 1.3h, 1.4h, 1.5h, 1.6h, 1.7h, 1.8h, 1.9h, 2h, 2.1h, 2.2h, 2.3h, 2.4h, 2.5h, 2.6h, 2.7h, 2.8h, 2.9h or 3h, but is not limited to the listed values, and other values not listed in the range are also applicable.
[0052] Preferably, the third sintering is sintering at 1000-1100° C. for 4-8 hours in a mixed atmosphere with an oxygen content of 19-21% by volume.
[0053] In the present invention, the volume percentage of oxygen in the mixed atmosphere of the third sintering is 19-21%, for example, it can be 19%, 19.1%, 19.2%, 19.3%, 19.4%, 19.5%, 19.6%, 19.7%, 19.8%, 19.9%, 20%, 20.1%, 20.2%, 20.3%, 20.4%, 20.5%, 20.6%, 20.7%, 20.8%, 20.9% or 21%, etc., but is not limited to the listed values, and other values not listed in the range are also applicable.
[0054] In the present invention, the temperature of the third sintering is 1000-1100°C, for example, it can be 1000°C, 1010°C, 1020°C, 1030°C, 1040°C, 1050°C, 1060°C, 1070°C, 1080°C, 1090°C or 1100°C, but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0055] In the present invention, the time of the third sintering is 4-8h, for example, it can be 4h, 4.2h, 4.4h, 4.6h, 4.8h, 5h, 5.2h, 5.4h, 5.6h, 5.8h, 6h, 6.2h, 6.4h, 6.6h, 6.8h, 7h, 7.2h, 7.4h, 7.6h, 7.8h or 8h, but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0056] As a preferred technical solution of the present invention, the preparation method comprises:
[0057] Prepare main ingredients and auxiliary ingredients according to the formula;
[0058] The main component material is ball-milled, dried and pre-calcined in sequence, then mixed with the auxiliary component material, sand-milled, and dried to obtain a ferrite mixture;
[0059] The obtained ferrite mixture is heat-treated in sequence, and then mixed with a binder and granulated to obtain ferrite granules, and then sintered in a mixed atmosphere and cooled to obtain a manganese-zinc ferrite material;
[0060] The ball milling method is wet ball milling; the mass ratio of the material to the grinding ball in the ball mill is 1:(7-8); the ball milling time is 30-50 minutes; the pre-burning temperature is 700-800°C; the pre-burning time is 2-3 hours; the sand milling method is wet sand milling; the sand milling time is 70-90 minutes; the heat treatment temperature is 700-850°C; the heat treatment time is 3-3.5 hours; the adhesive includes polyvinyl alcohol; the amount of the adhesive added is 8-10% of the mass of the ferrite mixture; the mixed atmosphere includes protective gas and oxygen, and the volume percentage of oxygen is 3-21%; the protective gas includes one or a combination of at least two of nitrogen, helium, neon or argon;
[0061] The sintering includes a second sintering, a third sintering and a first sintering performed sequentially;
[0062] The second sintering is sintering at 600-700°C for 1-3h in a mixed atmosphere with an oxygen volume percentage of 19-21%; the third sintering is sintering at 1000-1100°C for 4-8h in a mixed atmosphere with an oxygen volume percentage of 19-21%; the first sintering is sintering at 1280-1350°C for 4-10h in a mixed atmosphere with an oxygen volume percentage of 3-8%.
[0063] Compared with the prior art solutions, the present invention has the following beneficial effects:
[0064] The technical solution of the present invention prepares a manganese-zinc ferrite material with high magnetic permeability, high Curie temperature, wide temperature, wide frequency and low temperature coefficient by limiting the main formula range and the auxiliary component range and controlling the low-temperature pre-sintering process and sintering process parameters, and realizes a manganese-zinc ferrite with high magnetic permeability, wide temperature and low temperature coefficient at low cost. Among them, within the temperature range of 0-60°C, the magnetic permeability has a lower temperature coefficient within the range of 15000-16000, the Curie temperature is ≥136°C, and the initial magnetic permeability (25°C, 10KHz, 100KHz) μi ≥15200. DETAILED DESCRIPTION
[0065] To better illustrate the present invention and facilitate understanding of the technical solution of the present invention, typical but non-limiting embodiments of the present invention are as follows:
[0066] Example 1
[0067] The designed formula is Fe2O3 52.21mol%, MnO 26.31mol%, ZnO 21.48mol%, the main components are accurately weighed, put into a ball mill (the mass ratio of material to grinding ball is 1:7.5, mix for 40min until uniform, put into an oven for drying, and pre-calcine at 750℃ for 2.5 hours to obtain a pre-calcined powder, and then the auxiliary components designed in the pre-calcined powder (the auxiliary components are calculated according to the total amount of the main components, i.e., based on the main components): Bi2O3 450ppm, CaCO3200ppm, MoO 200ppm, CoO 1000ppm;
[0068] Sand mill for 90 minutes in a sand mill, then dry and heat treat at 750°C for 3.2 hours. Then mix 8wt% polyvinyl alcohol and the heat treated material to obtain ferrite particles and sieve. The ferrite particles are pressed into blanks with a size of H25×15×8 by a press, sintered at 600°C for 2 hours under the condition of N2 controlling the oxygen content (the gas is composed of oxygen and nitrogen) to 21vol%, sintered at 1100°C for 6 hours under the condition of N2 controlling the oxygen content (the gas is composed of oxygen and nitrogen) to 21vol%, and then sintered at 1300°C for 7 hours under the condition of N2 controlling the oxygen content (the gas is composed of oxygen and nitrogen) to 5.5vol%, cooled under the equilibrium oxygen partial pressure, and the powder core is tested.
[0069] The properties of the obtained materials are shown in Table 1.
[0070] Example 2
[0071] The designed formula is Fe2O3 51.10mol%, MnO 26.44mol%, ZnO 22.46mol%, the main components are accurately weighed, ball milled (the mass ratio of material to grinding ball is 1:7) and mixed for 30 minutes, put into an oven for drying, and pre-calcined at 700℃ for 3 hours to obtain a pre-calcined material, and auxiliary components are added to the pre-calcined material (auxiliary components are calculated based on the total amount of main components): CaCO3 400ppm, Bi2O3 600ppm, MoO 200ppm, CoO 1500ppm;
[0072] Sand mill for 70 minutes in a sand mill, then dry and heat treat at 850℃ for 3 hours. Then mix 8wt% polyvinyl alcohol with the heat-treated material to obtain ferrite particles and sieve. The ferrite particles are pressed into blanks with a size of H25×15×8 by a press, sintered at 600℃ for 3 hours under the condition of N2 controlling the oxygen content (gas consisting of oxygen and nitrogen) to be 19vol%, sintered at 1000℃ for 4 hours under the condition of N2 controlling the oxygen content (gas consisting of oxygen and nitrogen) to be 19vol%, and then sintered at 1340℃ for 4 hours under the condition of N2 controlling the oxygen content (gas consisting of oxygen and nitrogen) to be 3vol%, cooled under the equilibrium oxygen partial pressure, and the powder core is tested.
[0073] The properties of the obtained materials are shown in Table 1.
[0074] Example 3
[0075] The designed formula is Fe2O3 52.32mol%, MnO 26.48mol%, ZnO 21.20mol%, the main components are accurately weighed, ball milled in a ball mill (the mass ratio of material to grinding ball is 1:8) and mixed for 50 minutes, put into an oven for drying and pre-calcined at 800℃ for 2 hours to obtain a pre-calcined material, and auxiliary components are added to the pre-calcined material (auxiliary components are calculated based on the total amount of main components): CaCO3 200ppm, Bi2O3 600ppm, MoO 200ppm, CoO 1500ppm;
[0076] Sand mill for 90 minutes, then dry and heat treat at 700℃ for 3.5h, then spray granulate to obtain ferrite particles and sieve. Ferrite particles are pressed into blanks with a size of H25×15×8 by a press, sintered at 700℃ for 1 hour under the condition of N2 controlling oxygen content (gas composed of oxygen and nitrogen) to 20vol%, sintered at 1100℃ for 8 hours under the condition of N2 controlling oxygen content (gas composed of oxygen and nitrogen) to 20vol%, then sintered at 1280℃ for 10 hours under the condition of N2 controlling oxygen content (gas composed of oxygen and nitrogen) to 8vol%, cooled under balanced oxygen partial pressure, and powder cores are obtained for testing.
[0077] The properties of the obtained materials are shown in Table 1.
[0078] Example 4
[0079] The only difference from Example 1 is that the second sintering, ie, sintering at 600° C. for 2 hours in N 2 with an oxygen content of 21 vol % (the gas consists of oxygen and nitrogen), is not performed.
[0080] The properties of the obtained materials are shown in Table 1.
[0081] Example 5
[0082] The only difference from Example 1 is that the third sintering is not performed, that is, the sintering at 1100° C. for 6 hours in N2 with an oxygen content controlled to 21 vol% (the gas consists of oxygen and nitrogen) is not performed.
[0083] The properties of the obtained materials are shown in Table 1.
[0084] Example 6
[0085] The only difference from Example 1 is that the second sintering and the third sintering are not carried out, that is, the sintering at 600°C for 2 hours in the condition of N2 controlling the oxygen content (the gas is composed of oxygen and nitrogen) to be 21 vol% is not carried out, and the sintering at 1100°C for 6 hours in the condition of N2 controlling the oxygen content (the gas is composed of oxygen and nitrogen) to be 21 vol% is not carried out.
[0086] The properties of the obtained materials are shown in Table 1.
[0087] Example 7
[0088] The only difference from Example 1 is that the auxiliary components do not contain MoO.
[0089] The properties of the obtained materials are shown in Table 1.
[0090] Example 8
[0091] The only difference from Example 1 is that CoO is replaced by an equal amount of Co2O3.
[0092] The properties of the obtained materials are shown in Table 1.
[0093] Example 9
[0094] The only difference from Example 1 is that CaCO3 is replaced by an equal amount of CaO.
[0095] The properties of the obtained materials are shown in Table 1.
[0096] Example 10
[0097] The only difference from Example 1 is that the content of ZnO is adjusted to 12 mol %.
[0098] The properties of the obtained materials are shown in Table 1.
[0099] In the above embodiment, the performance test of the obtained material is to wrap the sample around a wire (with a diameter of 0.35 mm) for 10 turns and put it into a high and low temperature oven for gradient heating to the set temperature (0°C, 25°C, 40°C, 60°C). After keeping each section warm for 30 minutes, the test is performed using a CH3302 LCR testing device.
[0100] Table 1
[0101]
[0102]
[0103] It can be seen from the results of the above embodiments that the manganese-zinc ferrite material provided by the present invention can obtain a manganese-zinc ferrite material with high magnetic permeability, high Curie temperature (≥135°C), wide temperature, wide frequency, and low temperature coefficient characteristics through the main formula range and the auxiliary component range. Among them, the cobalt element is added as an auxiliary agent, the content of Fe in the main formula is reduced, and the proportion of iron, manganese, and zinc is strictly controlled to ensure high magnetic permeability. Furthermore, a reasonable proportion of cobalt element and iron element after sintering in the main component is added, and the two peak positions are adjusted to flatten the temperature curve, so that μi (25°C-60°C) reaches 15000-16000 and has a lower temperature coefficient.
[0104] It is stated that the present invention illustrates the detailed structural features of the present invention through the above embodiments, but the present invention is not limited to the above detailed structural features, that is, it does not mean that the present invention must rely on the above detailed structural features to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the components selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
[0105] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.
[0106] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.
[0107] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.
Claims
1. A manganese-zinc ferrite material, characterized in that: The manganese-zinc ferrite material comprises a main component and an auxiliary component; The main components include ZnO 19.6-21.48 mol%, MnO2 6.02-29.52 mol%, and the balance is Fe2O3 in terms of molar percentage; The auxiliary components include: CaCO3 100-2000ppm, Bi2O3 200-2000ppm, MoO100-2000ppm, CoO100-1500ppm, based on the main component.
2. The manganese-zinc ferrite material according to claim 1, characterized in that: The manganese-zinc ferrite material comprises a main component and an auxiliary component; The main components include ZnO 20-21.2mol%, MnO 27-28mol%, and the balance is Fe2O3 in terms of molar percentage; The auxiliary components include: CaCO3 200-400ppm, Bi2O3 450-600ppm, MoO200-800ppm, CoO 1000-1500ppm, based on the main component.
3. A method for preparing the manganese-zinc ferrite material as claimed in claim 1 or 2, characterized in that: The preparation method comprises: Prepare main ingredients and auxiliary ingredients according to the formula; The main component material is ball-milled, dried and pre-calcined in sequence, then mixed with the auxiliary component material, sand-milled, and dried to obtain a ferrite mixture; The obtained ferrite mixture is heat-treated in sequence, and then mixed with a binder and granulated to obtain ferrite particles, which are sintered in a mixed atmosphere and then cooled to obtain a manganese-zinc ferrite material.
4. The preparation method according to claim 3, characterized in that: The ball milling method is wet ball milling; Preferably, the mass ratio of the material to the grinding balls in the ball mill is 1:(7-8); Preferably, the ball milling time is 30-50 min; Preferably, the pre-burning temperature is 700-800°C; Preferably, the pre-burning time is 2-3 hours.
5. The preparation method according to claim 3 or 4, characterized in that: The sanding method is wet sanding; Preferably, the sanding time is 70-90 min.
6. The preparation method according to any one of claims 3 to 5, characterized in that: The temperature of the heat treatment is 700-850°C; Preferably, the heat treatment time is 3-3.5h.
7. The preparation method according to any one of claims 3 to 6, characterized in that: The adhesive includes polyvinyl alcohol; Preferably, the amount of the adhesive added is 8-10% of the mass of the ferrite mixture.
8. The preparation method according to any one of claims 3 to 7, characterized in that: The mixed atmosphere includes protective gas and oxygen, and the volume percentage of oxygen is 3-21%; Preferably, the protective gas includes one or a combination of at least two of nitrogen, helium, neon or argon.
9. The preparation method according to any one of claims 3 to 8, characterized in that: The sintering includes a first sintering; Preferably, the first sintering is sintering at 1280-1350° C. for 4-10 h in a mixed atmosphere with an oxygen volume percentage of 3-8%; Preferably, the first sintering further includes a second sintering and a third sintering performed in sequence before the first sintering; Preferably, the second sintering is sintering at 600-700° C. for 1-3 h in a mixed atmosphere with an oxygen volume percentage of 19-21%; Preferably, the third sintering is sintering at 1000-1100° C. for 4-8 hours in a mixed atmosphere with an oxygen content of 19-21% by volume.
10. The preparation method according to any one of claims 3 to 9, characterized in that: The preparation method comprises: Prepare main ingredients and auxiliary ingredients according to the formula; The main component material is ball-milled, dried and pre-calcined in sequence, then mixed with the auxiliary component material, sand-milled, and dried to obtain a ferrite mixture; The obtained ferrite mixture is heat-treated in sequence, and then mixed with a binder and granulated to obtain ferrite granules, and then sintered in a mixed atmosphere and cooled to obtain a manganese-zinc ferrite material; The ball milling method is wet ball milling; the mass ratio of the material to the grinding ball in the ball mill is 1:(7-8); the ball milling time is 30-50 minutes; the pre-burning temperature is 700-800°C; the pre-burning time is 2-3 hours; the sand milling method is wet sand milling; the sand milling time is 70-90 minutes; the heat treatment temperature is 700-850°C; the heat treatment time is 3-3.5 hours; the adhesive includes polyvinyl alcohol; the amount of the adhesive added is 8-10% of the mass of the ferrite mixture; the mixed atmosphere includes protective gas and oxygen, and the volume percentage of oxygen is 3-21%; the protective gas includes one or a combination of at least two of nitrogen, helium, neon or argon; The sintering includes a second sintering, a third sintering and a first sintering performed sequentially; The second sintering is sintering at 600-700°C for 1-3h in a mixed atmosphere with an oxygen volume percentage of 19-21%; the third sintering is sintering at 1000-1100°C for 4-8h in a mixed atmosphere with an oxygen volume percentage of 19-21%; the first sintering is sintering at 1280-1350°C for 4-10h in a mixed atmosphere with an oxygen volume percentage of 3-8%.
Citation Information
Patent Citations
High-magnetic-permeability ferrite material
CN103011791A
High-frequency high-impedance manganese-zinc ferrite material and preparation method thereof
CN111892395A
High-permeability, high-frequency, high-impedance and high-Curie-temperature manganese-zinc ferrite material and preparation method thereof
CN112321293A
Broadband wide-temperature high-permeability Mn-Zn ferrite material as well as preparation method and application thereof
CN112645702A
Mn-Zn ferrite material and preparation method thereof
CN113443906A