Preparation method of IGZO target material
By using ball milling process and molding-cold isostatic pressing process in the preparation of IGZO targets, combined with spray drying, the problem of insufficient density of IGZO targets in the prior art was solved, and a high-density target preparation was achieved , improves the stability and performance of the film.
Patent Information
- Application Number
- CN202411168325.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-12
AI Technical Summary
The insufficient density of existing IGZO targets leads to poor film quality in the RF magnetron sputtering process, affecting the performance of electronic devices.
Two batches of slurries with different solid contents were prepared in the ball milling process, and particles with different average particle sizes were obtained by spray drying. After mixing, the target material blank was prepared by molding-cold isostatic pressing process, and then sintered. , improve the density of the target material.
Effectively reduce particle gaps, increase the density of the blank after static pressure and the density of the target after sintering, reaching a relative density of more than 99.5%, ensuring the stability and high quality of the film.
Smart Images

Figure CN118930246A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of ceramic target materials, and in particular to a method for preparing an IGZO target material. Background Art
[0002] IGZO (Indium Gallium Zinc Oxide) target is a material used for depositing thin films, commonly used in electronic devices such as liquid crystal displays (LCDs) and organic light-emitting diodes (OLEDs). The density of IGZO targets is a key parameter to measure their quality and performance. High density means that the target has fewer defects and low porosity during the manufacturing process, thus providing more uniform and stable thin film deposition. Generally speaking, the density of IGZO targets should reach more than 99.9% to ensure stability and high-quality film formation during the deposition process.
[0003] IGZO targets are mainly used in the RF magnetron sputtering process to deposit IGZO thin films on substrates. IGZO thin films are widely used in displays and other electronic devices due to their excellent electron mobility, low power consumption and high transparency. The main components of IGZO include indium (In), gallium (Ga) and zinc (Zn), and its oxide form has good conductivity and stability.
[0004] The preparation of IGZO targets usually involves the mixing of high-purity raw materials and high-temperature sintering processes to form uniform and dense target blocks. High-density IGZO targets can effectively reduce film quality problems caused by target defects during sputtering, improve the efficiency of the deposition process and the performance of the film. How to improve the density of the target by optimizing the selection of IGZO target raw materials and process conditions has become a problem that needs to be solved urgently. Summary of the invention
[0005] In order to solve the problems and shortcomings in the prior art, the present invention provides a method for preparing an IGZO target material, which reduces the gaps between particles and increases the loose density, thereby increasing the density of the green blank after static pressing and the density of the target material after sintering.
[0006] Specifically, the present invention provides a method for preparing an IGZO target, comprising the following steps:
[0007] Step 1, mixing In2O3 powder, ZnO powder and Ga2O3 powder in a molar mass ratio of 1:2:1 and preparing a first batch of slurry and a second batch of slurry by ball milling, wherein the solid content of the first batch of slurry is 55-67wt%, and the solid content of the second batch of slurry is 46-55wt%;
[0008] Step 2, drying and granulating the first batch of slurry and the second batch of slurry respectively to prepare a first batch of particles and a second batch of particles with different average particle sizes, wherein the average particle size of the first batch of particles is less than or equal to 21 μm, and the average particle size of the second batch of particles is greater than or equal to 3 μm;
[0009] Step 3, mixing the first batch of particles with the second batch of particles and preparing a target blank by molding-cold isostatic pressing;
[0010] Step 4, preparing an IGZO target material by sintering the target material blank obtained in step 3.
[0011] Preferably, in step 1, when preparing the first batch of slurry and the second batch of slurry, a binder and a dispersant are added, the binder content is 0.8-1.2wt%, and the dispersant content is 0.3wt-2wt%.
[0012] Preferably, the binder is at least one of polyvinyl alcohol and polyethylene glycol.
[0013] Preferably, the dispersant is polyvinyl pyrrolidone.
[0014] Preferably, in step 2, granulation is performed by spray drying;
[0015] When the first batch of slurry is dried and granulated: the compressed air flow rate is 1.3m 3 / min-1.7m 3 / min, slurry supply rate is 10ml / min-13ml / min, and drying temperature is 180℃-220℃;
[0016] When the second batch of slurry is dried and granulated: the compressed air flow rate is 1.9m 3 / min-2.5.m 3 / min, the slurry supply rate is 7ml / min-9ml / min, and the drying temperature is 180℃-220℃.
[0017] Preferably, in step 2, the average particle size of the first batch of particles is 15 μm-21 μm, and the average particle size of the second batch of particles is 3 μm-5 μm.
[0018] Preferably, in step 3, the mass ratio of the first batch of particles to the second batch of particles is 4:10-7:10.
[0019] Compared with the prior art, the beneficial effect of the present invention lies in that: the present invention prepares two batches of slurry with different solid contents in the ball milling process, and uses the two batches of slurry for granulation respectively, the average diameters of the particles obtained by granulation are different, and the diameter of the batch of particles with a larger average diameter does not exceed 21 μm, which can avoid serious depressions in the formed particles, and the diameter of the batch of particles with a smaller average diameter is not less than 3 microns, which can avoid the disadvantage of poor fluidity of the formed particles; the two batches with different average diameters can reduce the gap between the particles after mixing, improve the loose density, and improve the density of the green billet after static pressing and the density of the target material after sintering. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 This is a flow chart of the method for preparing the IGZO target material of Example 1 of the present invention. DETAILED DESCRIPTION
[0021] Next, a method for preparing an IGZO target material according to an embodiment of the present invention is described. In the description of this embodiment, it should be understood that the terms "first" and "second" are used for descriptive purposes only, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Thus, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features, that is, include one or more of the features. In the description of the present invention, the meaning of "multiple" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined. When a feature "includes or contains" one or some of the features it covers, unless otherwise specifically described, this indicates that other features are not excluded and may further include other features.
[0022] In the description of the present embodiment, the description with reference to the terms "one embodiment", "some embodiments", "illustrative embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials, or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials, or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.
[0023] The present invention provides a method for preparing an IGZO target material, as shown in the following Figure 1 As shown, the following steps are included:
[0024] Step 1, respectively preparing a first batch of slurry and a second batch of slurry formed by mixing In2O3 powder, ZnO powder, and Ga2O3 powder, wherein the molar mass ratio of In2O3 powder, ZnO powder, and Ga2O3 powder is 1:2:1, the solid content of the first batch of slurry is 55-67wt%, and the solid content of the second batch of slurry is 46-55wt%;
[0025] Step 2, drying and granulating the first batch of slurry and the second batch of slurry to prepare the first batch of particles and the second batch of particles with different average particle sizes, wherein the average particle size of the first batch of particles is less than or equal to 21 μm, and the average particle size of the second batch of particles is greater than or equal to 3 μm;
[0026] Step 3, mixing the first batch of particles with the second batch of particles and preparing a target blank by molding-cold isostatic pressing;
[0027] Step 4, preparing an IGZO target material by sintering the target material blank obtained in step 3.
[0028] Preferably, in step 1, when preparing the first batch of slurry and the second batch of slurry, a binder and a dispersant need to be added, the binder content is 0.8-1.2wt%, and the dispersant content is 0.3wt-2wt%.
[0029] Preferably, the binder is at least one of polyvinyl alcohol and polyethylene glycol.
[0030] Preferably, the dispersant is polyvinyl pyrrolidone.
[0031] Preferably, in step 2, the first batch of slurry and the second batch of slurry are dried and granulated by a spray method. When the first batch of slurry is dried and granulated: the compressed air flow rate is 1.3m 3 / min-1.7m 3 / min, the slurry supply rate is 10ml / min-13ml / min, and the drying temperature is 180℃-220℃; when the second batch of slurry is dried and granulated: the compressed air flow rate is 1.9m 3 / min-2.5.m 3 / min, the slurry supply rate is 7ml / min-9ml / min, and the drying temperature is 180℃-220℃.
[0032] Preferably, in step 2, the average particle size of the first batch of particles is 15 μm-21 μm, and the average particle size of the second batch of particles is 3 μm-5 μm.
[0033] Preferably, in step 3, the mass ratio of the first batch of particles to the second batch of particles is 4:10-7:10.
[0034] Preferably, in step 1, the first batch of slurry and the second batch of slurry are prepared by ball milling process.
[0035] Example 1
[0036] A method for preparing an IGZO target comprises the following steps:
[0037] Step 1: Take In2O3 powder, ZnO powder and Ga2O3 powder in a molar mass ratio of 1:2:1 and mix them evenly.
[0038] Take part of the mixed powder, add 0.5wt% dispersant, 1.1wt% binder, 0.02wt% defoamer and plasma water prepared in proportion, add them to a ball mill and mill for 48 hours to obtain the first batch of nano powder slurry with a solid content of 63wt%;
[0039] Part of the mixed powder was added to a ball mill with 0.5 wt% dispersant, 0.8 wt% binder, 0.02 wt% defoamer and plasma water prepared in proportion, and milled for 48 hours to obtain a second batch of nano powder slurry with a solid content of 46 wt%.
[0040] The dispersant is polyvinyl pyrrolidone; the binder is polyvinyl alcohol; the defoamer is n-butanol; and the particle sizes of the first batch of nano-powder slurry and the second batch of nano-powder slurry after ball milling are both less than 0.5 μm.
[0041] Step 2, drying and granulating the first batch of nano-powder slurry and the second batch of nano-powder slurry to prepare the first batch of particles and the second batch of particles with different average particle sizes:
[0042] The first batch of nano powder slurry was granulated by spray drying. The supply rate of nano powder slurry was 11ml / min and the compressed air flow rate was 1.7m / min. 3 / min, the drying temperature is 180°C; the average particle size of the first batch of particles prepared is 15 μm, wherein D10=4.3 μm, D90=22.8 μm.
[0043] The second batch of nano powder slurry was granulated by spray drying. The supply rate of nano powder slurry was 7 ml / min and the compressed air flow rate was 2.5 m / min. 3 / min, the drying temperature is 220°C; the average particle size of the second batch of particles prepared is 3 μm, wherein D10 = 0.9 μm, D90 = 6.1 μm;
[0044] Step 3: Mix the first batch of particles with the second batch of particles in a mass ratio of 4.3:10. The bulk density after mixing is 2.06 g / cm3 , the loose relative density is 32.29%; the IGZO green billet is prepared by the molding-cold isostatic pressing process, the molding pressure is 52MPa, the holding time is 5min, and the re-pressing pressure is 250Mpa. The density of the green billet after re-pressing is 3.50g / cm 3 , the relative density of the green compact after re-pressing is 54.86%;
[0045] Step 4, sintering the IGZO blank prepared in step 3, the heating rate of the first sintering section is 0.5℃ / min, the temperature is heated to 160℃ and then kept warm for 2H, the heating rate of the second sintering section is 2.3℃ / min, the temperature is heated to 800℃ and then kept warm for 8H, the heating rate of the third sintering section is 2.3℃ / min, the temperature is heated to 1380℃ and then kept warm for 3H, and the IGZO target is prepared after cooling.
[0046] The target material obtained in Example 1 has a relative density of 99.52% and has no cracks or hidden scratches.
[0047] Example 2
[0048] A method for preparing an IGZO target comprises the following steps:
[0049] Step 1: Take In2O3 powder, ZnO powder and Ga2O3 powder in a molar mass ratio of 1:2:1 and mix them evenly.
[0050] Take part of the mixed powder, add 2wt% dispersant, 1.1wt% binder, 0.02wt% defoamer and plasma water prepared in proportion, add them to a ball mill and mill for 48 hours to obtain the first batch of nano powder slurry with a solid content of 63wt%;
[0051] Part of the mixed powder was added to a ball mill with 0.3wt% dispersant, 0.8wt% binder, 0.02wt% defoamer and plasma water prepared in proportion, and milled for 48 hours to obtain a second batch of nano powder slurry with a solid content of 52wt%.
[0052] The dispersant is polyvinyl pyrrolidone; the binder is polyvinyl alcohol; the defoamer is n-butanol; and the particle sizes of the first batch of nano-powder slurry and the second batch of nano-powder slurry after ball milling are both less than 0.5 μm.
[0053] Step 2, drying and granulating the first batch of nano-powder slurry and the second batch of nano-powder slurry to prepare the first batch of particles and the second batch of particles with different average particle sizes:
[0054] The first batch of nano powder slurry was granulated by spray drying. The supply rate of nano powder slurry was 11ml / min and the compressed air flow rate was 1.7m / min. 3 / min, the drying temperature is 190°C; the average particle size of the first batch of particles prepared is 15 μm, wherein D10=4.3 μm, D90=22.8 μm;
[0055] The second batch of nano powder slurry was granulated by spray drying. The supply rate of nano powder slurry was 7 ml / min and the compressed air flow rate was 2.5 m / min. 3 / min, the drying temperature is 220°C; the average particle size of the second batch of particles prepared is 5 μm, wherein D10=1.4 μm, D90=12.7 μm;
[0056] Step 3: Mix the first batch of particles with the second batch of particles in a mass ratio of 6:10. The bulk density after mixing is 1.92 g / cm 3 , the loose relative density is 30.10%; the IGZO green billet is prepared by molding-cold isostatic pressing process, the molding pressure is 52MPa, the holding time is 5min, and the re-pressing pressure is 250Mpa. The density of the green billet after re-pressing is 3.43g / cm 3 , the relative density of the green compact after re-pressing is 53.77%;
[0057] Step 4: The sintering process is the same as that in Example 1.
[0058] The target material obtained in Example 2 has a relative density of 99.47% and has no cracks or hidden scratches.
[0059] Example 3
[0060] A method for preparing an IGZO target comprises the following steps:
[0061] Step 1: Take In2O3 powder, ZnO powder and Ga2O3 powder in a molar mass ratio of 1:2:1 and mix them evenly.
[0062] Take part of the mixed powder, add 1.5wt% dispersant, 1.2wt% binder, 0.02wt% defoamer and plasma water prepared in proportion, add them to a ball mill and mill for 48 hours to obtain the first batch of nano powder slurry with a solid content of 66wt%;
[0063] Part of the mixed powder was added to a ball mill with 2 wt% dispersant, 0.8 wt% binder, 0.02 wt% defoamer and plasma water prepared in proportion, and milled for 48 hours to obtain a second batch of nanopowder slurry with a solid content of 46 wt%.
[0064] The dispersant is polyvinyl pyrrolidone; the binder is polyvinyl alcohol; the defoamer is n-butanol; and the particle sizes of the first batch of nano-powder slurry and the second batch of nano-powder slurry after ball milling are both less than 0.5 μm.
[0065] Step 2, drying and granulating the first batch of nano-powder slurry and the second batch of nano-powder slurry to prepare the first batch of particles and the second batch of particles with different average particle sizes:
[0066] The first batch of nano powder slurry was granulated by spray drying. The supply rate of nano powder slurry was 12ml / min and the compressed air flow rate was 1.6m / min. 3 / min, the drying temperature is 200°C; the average particle size of the first batch of particles prepared is 21 μm, wherein D10=6.9 μm, D90=39.8 μm;
[0067] The second batch of nano powder slurry was granulated by spray drying, the supply rate of the nano powder slurry was 7 ml / min, the compressed air flow rate was 2.53 / min, and the drying temperature was 190°C; the average particle size of the second batch of particles prepared was 3 μm, wherein D10 = 0.9 μm, D90 = 6.1 μm;
[0068] Step 3: Mix the first batch of particles with the second batch of particles in a mass ratio of 4:10. The bulk density after mixing is 2.21 g / cm 3 , the loose relative density is 34.64%; the IGZO green billet is prepared by the molding-cold isostatic pressing process, the molding pressure is 52MPa, the holding time is 5min, and the re-pressing pressure is 250Mpa. The density of the green billet after re-pressing is 3.61g / cm 3 , the relative density of the green compact after re-pressing is 56.59%;
[0069] Step 4: The sintering process is the same as that in Example 1.
[0070] The target material obtained in Example 3 has a relative density of 99.67% and has no cracks or hidden scratches.
[0071] Example 4
[0072] A method for preparing an IGZO target comprises the following steps:
[0073] Step 1: Take In2O3 powder, ZnO powder and Ga2O3 powder in a molar mass ratio of 1:2:1 and mix them evenly.
[0074] Take part of the mixed powder, add 0.3wt% dispersant, 1.2wt% binder, 0.02wt% defoamer and plasma water prepared in proportion, add them to a ball mill and mill for 48 hours to obtain the first batch of nano powder slurry with a solid content of 66wt%;
[0075] Part of the mixed powder was added to a ball mill with 1.2 wt% dispersant, 0.8 wt% binder, 0.02 wt% defoamer and plasma water prepared in proportion, and milled for 48 hours to obtain a second batch of nano powder slurry with a solid content of 52 wt%.
[0076] The dispersant is polyvinyl pyrrolidone; the binder is polyvinyl alcohol; the defoamer is n-butanol; and the particle sizes of the first batch of nano-powder slurry and the second batch of nano-powder slurry after ball milling are both less than 0.5 μm.
[0077] Step 2, drying and granulating the first batch of nano-powder slurry and the second batch of nano-powder slurry to prepare the first batch of particles and the second batch of particles with different average particle sizes:
[0078] The first batch of nano powder slurry was granulated by spray drying. The supply rate of nano powder slurry was 12ml / min and the compressed air flow rate was 1.6m / min. 3 / min, the drying temperature is 220°C; the average particle size of the first batch of particles prepared is 21 μm, wherein D10=6.9 μm, D90=39.8 μm;
[0079] The second batch of nano powder slurry was granulated by spray drying. The supply rate of nano powder slurry was 9 ml / min and the compressed air flow rate was 2.5 m / min. 3 / min, the drying temperature is 210°C; the average particle size of the second batch of particles prepared is 5 μm, wherein D10=1.4 μm, D90=12.7 μm;
[0080] Step 3: Mix the first batch of particles with the second batch of particles in a mass ratio of 7:10. The bulk density after mixing is 2.13 g / cm 3 , the loose relative density is 33.39%; the IGZO green billet is prepared by the molding-cold isostatic pressing process, the molding pressure is 52MPa, the holding time is 5min, and the re-pressing pressure is 250Mpa. The density of the green billet after re-pressing is 3.58g / cm 3 , the relative density of the green compact after re-pressing is 56.12%;
[0081] Step 4: The sintering process is the same as that in Example 1.
[0082] The target material obtained in Example 4 has a relative density of 99.58% and has no cracks or hidden scratches.
[0083] Example 5
[0084] A method for preparing an IGZO target comprises the following steps:
[0085] Step 1: Take In2O3 powder, ZnO powder and Ga2O3 powder in a molar mass ratio of 1:2:1 and mix them evenly.
[0086] Take part of the mixed powder, add 0.3wt% dispersant, 1.1wt% binder, 0.02wt% defoamer and plasma water prepared in proportion, add them to a ball mill and mill for 48 hours to obtain the first batch of nano powder slurry with a solid content of 66wt%;
[0087] Part of the mixed powder was added to a ball mill with 1.2 wt% dispersant, 0.9 wt% binder, 0.02 wt% defoamer and plasma water prepared in proportion, and milled for 48 hours to obtain a second batch of nano powder slurry with a solid content of 56 wt%.
[0088] The dispersant is polyvinyl pyrrolidone; the binder is polyvinyl alcohol; the defoamer is n-butanol; and the particle sizes of the first batch of nano-powder slurry and the second batch of nano-powder slurry after ball milling are both less than 0.5 μm.
[0089] Step 2, drying and granulating the first batch of nano-powder slurry and the second batch of nano-powder slurry to prepare the first batch of particles and the second batch of particles with different average particle sizes:
[0090] The first batch of nano powder slurry was granulated by spray drying. The supply rate of nano powder slurry was 11ml / min and the compressed air flow rate was 1.7m / min. 3 / min, the drying temperature is 180°C; the average particle size of the first batch of particles prepared is 15 μm, wherein D10=4.3 μm, D90=22.8 μm;
[0091] The second batch of nano powder slurry was granulated by spray drying. The supply rate of nano powder slurry was 9 ml / min and the compressed air flow rate was 2.3 m / min. 3 / min, the drying temperature is 220°C; the average particle size of the second batch of particles prepared is 7.9 μm, wherein D10=2.8 μm, D90=16.2 μm;
[0092] Step 3: Mix the first batch of particles with the second batch of particles in a mass ratio of 7:10. The bulk density after mixing is 1.71 g / cm 3 , the loose relative density is 26.80%; the IGZO green billet is prepared by molding-cold isostatic pressing process, the molding pressure is 52MPa, the holding time is 5min, and the re-pressing pressure is 250Mpa. The density of the green billet after re-pressing is 2.99g / cm 3 , the relative density of the green compact after re-pressing is 46.87%;
[0093] Step 4: The sintering process is the same as that in Example 1.
[0094] The target material obtained in Example 5 has a relative density of 99.29% and has no cracks or hidden scratches.
[0095] Example 6
[0096] A method for preparing an IGZO target comprises the following steps:
[0097] Step 1: In2O3 powder, ZnO powder, and Ga2O3 powder are mixed uniformly according to a molar mass ratio of 1:2:1.
[0098] Take part of the mixed powder, add 0.3wt% dispersant, 1.0wt% binder, 0.02wt% defoamer and plasma water prepared in proportion, add them to a ball mill and mill for 48 hours to obtain the first batch of nano powder slurry with a solid content of 60wt%;
[0099] Part of the mixed powder was added to a ball mill with 1.2 wt% dispersant, 0.8 wt% binder, 0.02 wt% defoamer and plasma water prepared in proportion, and milled for 48 hours to obtain a second batch of nano powder slurry with a solid content of 52 wt%;
[0100] The dispersant is polyvinyl pyrrolidone; the binder is polyvinyl alcohol; the defoamer is n-butanol; and the particle sizes of the first batch of nano-powder slurry and the second batch of nano-powder slurry after ball milling are both less than 0.5 μm.
[0101] Step 2, drying and granulating the first batch of nano-powder slurry and the second batch of nano-powder slurry to prepare the first batch of particles and the second batch of particles with different average particle sizes:
[0102] The first batch of nano powder slurry was granulated by spray drying. The supply rate of nano powder slurry was 10ml / min and the compressed air flow rate was 2.0m 3 / min, the drying temperature is 200°C; the average particle size of the first batch of particles prepared is 13.7μm, wherein D10=3.7μm, D90=22μm;
[0103] The second batch of nano powder slurry was granulated by spray drying. The supply rate of nano powder slurry was 9 ml / min and the compressed air flow rate was 2.5 m / min. 3 / min, the drying temperature is 180°C; the average particle size of the second batch of particles prepared is 5.0 μm, wherein D10=1.4 μm, D90=12.7 μm;
[0104] Step 3: Mix the first batch of particles with the second batch of particles in a mass ratio of 7:10. The bulk density after mixing is 1.79 g / cm 3 , the loose relative density is 28.06%; the IGZO green billet is prepared by the molding-cold isostatic pressing process, the molding pressure is 52MPa, the holding time is 5min, and the re-pressing pressure is 250Mpa. The density of the green billet after re-pressing is 3.05g / cm 3 , the relative density of the green compact after re-pressing is 47.81%;
[0105] Step 4: The sintering process is the same as that in Example 1.
[0106] The target material obtained in Example 6 has a relative density of 99.33% and has no cracks or hidden scratches.
[0107] Comparative Example 1
[0108] Comparative Example 1 provides a one-step preparation method, which is a method for preparing a target material without mixing two batches of different slurries. The specific steps are as follows:
[0109] Step 1: Take and mix In2O3 powder, ZnO powder and Ga2O3 powder according to the molar mass ratio of 1:2:1.
[0110] Part of the mixed powder was added to a ball mill together with 0.5wt% dispersant, 1.0wt% binder, 0.02wt% defoamer and deionized water for 48 hours to obtain a nano powder slurry with a solid content of 60wt%; wherein the dispersant was polyvinyl alcohol; the binder was polyvinyl pyrrolidone; the defoamer was n-butanol; the powder particle size after ball milling was less than 0.5μm;
[0111] Step 2: Spray drying is used for granulation. The supply rate of nano powder slurry is 10 ml / min and the compressed air flow rate is 2.0 m / min. 3 / min, the drying temperature is 200°C; the average particle size of the prepared particles is 13.7μm, wherein D10=3.7μm, D90=22μm;
[0112] Step 3: The bulk density of the particles prepared in step 2 is 1.51 g / cm 3 The relative density after loose packing is 23.67%. The IGZO green billet is prepared by the molding-cold isostatic pressing process with a molding pressure of 52MPa, a holding time of 5min, and a re-pressing pressure of 250MPa. The density of the green billet after re-pressing is 2.84g / cm 3 , the relative density of the green compact after re-pressing is 44.52%;
[0113] Step 4 is the same as in Example 1.
[0114] The target material obtained in Comparative Example 1 has a relative density of 99.20% and has no cracks or hidden scratches.
[0115] Comparative Example 2
[0116] Comparative Example 2 provides a preparation method, wherein the particle size of the second batch of particles is less than 3 μm, and the specific steps are as follows:
[0117] Step 1: Take In2O3 powder, ZnO powder and Ga2O3 powder in a molar mass ratio of 1:2:1 and mix them evenly.
[0118] Take part of the mixed powder, add 0.5wt% dispersant, 1.1wt% binder, 0.02wt% defoamer and plasma water prepared in proportion, put them into a ball mill for 48 hours to obtain the first batch of nano powder slurry with a solid content of 63wt%.
[0119] Part of the mixed powders, 0.5wt% dispersant, 0.8wt% binder, 0.02wt% defoamer and plasma water prepared in proportion were added to a ball mill for 48 hours to obtain a second batch of nano powder slurry with a solid content of 44wt%;
[0120] Step 2, drying and granulating the first batch of nano-powder slurry and the second batch of nano-powder slurry to prepare the first batch of particles and the second batch of particles with different average particle sizes:
[0121] The first batch of nano powder slurry was granulated by spray drying. The supply rate of nano powder slurry was 11ml / min and the compressed air flow rate was 1.7m / min. 3 / min, the drying temperature is 180°C; the average particle size of the first batch of particles prepared is 15 μm, wherein D10=4.3 μm, D90=22.8 μm;
[0122] The second batch of nano powder slurry was granulated by spray drying. The supply rate of nano powder slurry was 7 ml / min and the compressed air flow rate was 2.5 m / min. 3 / min, the drying temperature is 220°C; the average particle size of the second batch of particles prepared is 2.8μm, wherein D10=0.7μm, D90=5.5μm.
[0123] In Comparative Example 2, the obtained particles have poor fluidity and serious powder agglomeration, and are not suitable for further sintering.
[0124] Comparative Example 3
[0125] Comparative Example 3 provides a preparation method, wherein the particle size of the first batch of particles is greater than 21 μm, and the specific steps are as follows:
[0126] Step 1: Take In2O3 powder, ZnO powder and Ga2O3 powder in a molar mass ratio of 1:2:1 and mix them evenly.
[0127] Take part of the mixed powder, add 0.5wt% dispersant, 1.2wt% binder, 0.02wt% defoamer and plasma water prepared in proportion, add them to a ball mill and mill for 48 hours to obtain the first batch of nano powder slurry with a solid content of 67wt%;
[0128] Part of the mixed powder was added to a ball mill with 0.5wt% dispersant, 0.8wt% binder, 0.02wt% defoamer and plasma water prepared in proportion, and milled for 48 hours to obtain a second batch of nano powder slurry with a solid content of 52wt%;
[0129] Step 2, drying and granulating the first batch of nano-powder slurry and the second batch of nano-powder slurry to prepare the first batch of particles and the second batch of particles with different average particle sizes:
[0130] The first batch of nano powder slurry was granulated by spray drying. The supply rate of nano powder slurry was 13ml / min and the compressed air flow rate was 1.5m 3 / min, the drying temperature is 180°C; the average particle size of the first batch of particles prepared is 23 μm, wherein D10=7.1 μm, D90=43 μm;
[0131] The second batch of nano powder slurry was granulated by spray drying. The supply rate of nano powder slurry was 9 ml / min and the compressed air flow rate was 2.5 m / min. 3 / min, the drying temperature is 220°C; the average particle size of the second batch of particles prepared is 5.0 μm, wherein D10=1.4 μm, D90=12.7 μm.
[0132] In Comparative Example 3, the first batch of particles obtained had serious hollow defects and were not suitable for further sintering.
[0133] The comparison of the bulk density, the green billet density after re-pressing and the target density after sintering in Examples 1-6 and Comparative Examples 1-3 is shown in Table 1.
[0134] Table 1. Density comparison in Examples 1-6 and Comparative Examples 1-3
[0135]
[0136] From the comparison of the data in the above table, we can see that:
[0137] The IGZO target material obtained by directly loosening, vibrating and sintering a single batch of particles has a low density of only 99.2%.
[0138] By mixing two batches of particles with different average particle sizes, loosening them and sintering them, a high-density IGZO target can be obtained.
[0139] However, when the average particle size of each batch is too small (less than 3 μm), D10=0.7 μm in the particle size distribution, and the particles at the submicron level will have obvious agglomeration and cracks will appear after sintering; when the average particle size of each batch is too large (less than 21 μm), it is difficult to adjust the parameters of the dry granulation method to keep the formed powder in a solid round shape, that is, the formed particles will have depressions and hollow defects.
[0140] Moreover, when the ratio of the average particle size of the two batches of particles used for mixing is smaller, the density of the IGZO target material prepared by the mixed particles is improved compared with that of Comparative Example 1, but the improvement is not obvious. Taking Examples 5 and 6 as examples, when the diameter of the second batch of particles with a smaller average particle size is greater than 5 μm, or the diameter of the first batch of particles with a larger average particle size is less than 15 μm, the density of the formed IGZO target material is less than 99.4%.
[0141] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any person skilled in the art can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.
Claims
1. A method for preparing an IGZO target material, It is characterized in that The following steps are involved: Step 1, using In with a molar mass ratio of 1:2:1 2 O 3 Powder, ZnO powder, Ga 2 O 3 After the powders are mixed, a first batch of slurry and a second batch of slurry are prepared by ball milling process, wherein the solid content of the first batch of slurry is 55-67wt%, and the solid content of the second batch of slurry is 46-55wt%; Step 2, drying and granulating the first batch of slurry and the second batch of slurry respectively to prepare a first batch of particles and a second batch of particles with different average particle sizes, wherein the average particle size of the first batch of particles is less than or equal to 21 μm, and the average particle size of the second batch of particles is greater than or equal to 3 μm; Step 3, mixing the first batch of particles with the second batch of particles and preparing a target blank by molding-cold isostatic pressing; Step 4: Prepare the target material blank by sintering process to obtain IGZO target material.
2. The method for preparing the IGZO target according to claim 1, It is characterized in that In the step 1, when preparing the first batch of slurry and the second batch of slurry, a binder and a dispersant are added; The content of the binder is 0.8wt%-1.2wt%, and the content of the dispersant is 0.3wt%-2wt%.
3. The method for preparing the IGZO target according to claim 2, It is characterized in that The binder is at least one of polyvinyl alcohol and polyethylene glycol.
4. The method for preparing the IGZO target according to claim 2, It is characterized in that The dispersant is polyvinyl pyrrolidone.
5. The method for preparing the IGZO target according to claim 1, It is characterized in that In the step 2, granulation is performed by spray drying; When the first batch of slurry is dried and granulated: the compressed air flow rate is 1.3m 3 / min-1.7m 3 / min, slurry supply rate is 10ml / min-13ml / min, and drying temperature is 180℃-220℃; When the second batch of slurry is dried and granulated: the compressed air flow rate is 1.9m 3 / min-2.5.m 3 / min, the slurry supply rate is 7ml / min-9ml / min, and the drying temperature is 180℃-220℃.
6. The method for preparing the IGZO target according to claim 1, It is characterized in that In the step 2, the average particle size of the first batch of particles is 15 μm-21 μm, and the average particle size of the second batch of particles is 3 μm-5 μm.
7. The method for preparing the IGZO target according to claim 1, It is characterized in that In step 3, the mass ratio of the first batch of particles to the second batch of particles is 4:10-7:10.
Citation Information
Patent Citations
High-performance ITO granulation powder preparation method
CN106082993A
Method for preparing indium tin oxide target material based on grain composition accumulation model
CN112811896A
Preparation method of IGZO sputtering target material
CN115124324A
Indium molybdenum praseodymium oxide target material and preparation method thereof
CN116143500A
Indium zinc oxide target material and preparation method thereof
CN116219375A