High-energy-storage-density lead-free ceramic capacitor material and preparation method thereof
Through the chemical ratio and preparation method of (1-x)(Na0.5Bi0.5TiO3)-x(Bi1/6Na1/6Ca1/6Sr1/6Nd1/6Li1/6)TiO3, the high energy storage density and preparation method of ceramic capacitor materials are solved. The challenge of high efficiency design achieves high performance, environmentally friendly and stable lead-free ceramic capacitors, suitable for the needs of modern electronic equipment.
Patent Information
- Application Number
- CN202410982990.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-12
AI Technical Summary
The prior art is difficult to have both high energy storage density and high efficiency design, and the chemical stability and environmental friendliness of ceramic capacitor materials are insufficient, making it difficult to meet the needs of modern electronic equipment for high power density and fast charging and discharge.
Using the chemical ratio of (1-x)(Na0.5Bi0.5TiO3)-x(Bi1/6Na1/6Ca1/6Sr1/6Nd1/6Li1/6)TiO3, by mixing Na2CO3, Bi2O3, TiO2 and Na2CO3, Bi2O3, CaCO3, The oxides such as SrCO3, Li2CO3, Nd2O3, TiO2 are ball milled and prefired to prepare high-energy storage density lead-free ceramic capacitor materials, and high-performance ceramics are formed through binder granulation, tablet forming, calcining and gold spraying steps. Capacitor.
Lead-free ceramic capacitors with high energy storage density (18.2J/cm3), high efficiency (85.6%) and high stability (20-120℃, 1-500Hz) are achieved. The materials are safe, environmentally friendly and suitable for large-scale production.
Smart Images

Figure CN118930253A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of dielectric energy storage ceramic applications, and in particular to a high energy storage density lead-free ceramic capacitor material and a preparation method thereof. Background Art
[0002] The rapid development of electronic information technology has accelerated the speed of upgrading and replacing electronic components. Energy storage devices of ceramic dielectric capacitors have become indispensable key devices for pulse power. The design and development of high energy storage density ceramic capacitor materials is a frontier hotspot in today's information age. With the requirements of human health and sustainable development, new demands have been put forward for energy storage ceramic materials. The development of green and efficient energy storage dielectric ceramic materials is imperative in the field of dielectric capacitors.
[0003] Energy storage capacitors are considered an important component of pulse power systems due to their high power density, fast charge and discharge capabilities, and excellent chemical stability. However, how to achieve both high energy storage density and high efficiency is a major challenge. Reasonable material design is the key and core problem in building ceramic materials with high-efficiency energy storage performance. Summary of the invention
[0004] The object of the present invention is to provide a high energy storage density lead-free ceramic capacitor material and a preparation method thereof, wherein the prepared lead-free ceramic capacitor has ultra-high density, high efficiency and high stability.
[0005] In one aspect of the present invention, a high energy storage density lead-free ceramic capacitor material is provided. According to an embodiment of the present invention, the material is (1-x)(Na 0.5 Bi 0.5 TiO3)-x(Bi 1 / 6 Na 1 / 6 Ca 1 / 6 Sr 1 / 6 Nd 1 / 6 Li 1 / 6 )TiO3 is stoichiometrically proportioned, wherein x is the number of moles, and the value range of x is 0≤x≤0.55.
[0006] In another aspect of the present invention, the present invention provides a method for preparing a high energy storage density lead-free ceramic capacitor material. According to an embodiment of the present invention, the method comprises the following steps:
[0007] (1) Na2CO3, Bi2O3, and TiO2 are mixed, ball-milled, dried, and pre-calcined to obtain Na 0.5 Bi 0.5 TiO3 powder;
[0008] (2) Na2CO3, Bi2O3, CaCO3, SrCO3, Li2CO3, Nd2O3, and TiO2 are mixed, ball-milled, dried, and pre-calcined to obtain (Bi 1 / 6 Na 1 / 6 Ca 1 / 6 Sr 1 / 6 Nd 1 / 6 Li 1 / 6 )TiO3 powder;
[0009] (3) Put Na 0.5 Bi 0.5 TiO3 powder and (Bi 1 / 6 Na 1 / 6 Ca 1 / 6 Sr 1 / 6 Nd 1 / 6 Li 1 / 6 )TiO3 powder is mixed, ball-milled and dried to obtain the high energy storage density lead-free ceramic capacitor material.
[0010] In addition, the method for preparing a high energy storage density lead-free ceramic capacitor material according to the above embodiment of the present invention may also have the following additional technical features:
[0011] In some embodiments of the present invention, in step (1), the molar ratio of Na2CO3, Bi2O3 and TiO2 is 0.5:0.5:1, the pre-calcination temperature is 800-900°C, the pre-calcination time is 3-6h, and the heating rate is 3-5°C / min.
[0012] In some embodiments of the present invention, in the step (1), the molar ratio of Na2CO3, Bi2O3, CaCO3, SrCO3, Li2CO3, Nd2O3 and TiO2 is 1 / 6:1 / 6:1 / 6:1 / 6:1 / 6:1 / 6:1, the pre-firing temperature is 900-1000°C, the pre-firing time is 3-6h, and the heating rate is 3-5°C / min.
[0013] In some embodiments of the present invention, the ball milling uses anhydrous ethanol as the medium, zirconia balls as the ball milling beads, the mixed ball milling is 10-12 hours, anhydrous ethanol is used for discharging, the drying temperature is 60-80°C, and the drying time is 10-12 hours.
[0014] In another aspect of the present invention, the present invention provides a method for preparing a high energy storage density lead-free ceramic capacitor. According to an embodiment of the present invention, the method comprises the following steps:
[0015] (1) adding a binder to the high energy storage density lead-free ceramic capacitor material for granulation, and pressing into tablets to obtain a circular ceramic body;
[0016] (2) heating the round ceramic body to remove binder;
[0017] (3) calcining the round ceramic body after debinding to obtain lead-free ceramic;
[0018] (4) The lead-free ceramic surface is polished and cleaned, and then a gold electrode is sprayed on the surface to obtain the high energy storage density lead-free ceramic capacitor.
[0019] In addition, the method for preparing a high energy storage density lead-free ceramic capacitor according to the above embodiment of the present invention may also have the following additional technical features:
[0020] In some embodiments of the present invention, in step (1), the adhesive is a 4wt%-6wt% aqueous solution of polyvinyl alcohol, and the tableting is performed in a mold with a diameter of 8-12 mm.
[0021] In some embodiments of the present invention, in the step (2), the ceramic plastic body is heated for debinding at a temperature of 500-700° C. and the heat preservation time is 5-7 hours.
[0022] In some embodiments of the present invention, in step (3), the calcination temperature is 1150-1250° C., and the calcination time is 3-6 hours.
[0023] In some embodiments of the present invention, in step (4), 2000-10000 mesh sandpaper is used for polishing, and an ion sputtering device is used for gold spraying, and the gold spraying time is 60-120 seconds.
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] 1. Na 0.5 Bi 0.5 TiO3 has a complex phase structure and good dielectric, piezoelectric and ferroelectric properties, especially the higher P max (~40μC / cm 2 ), but pure Na 0.5 Bi 0.5 TiO3 ceramics have a large P r (~32uC / μC / cm 2 ) and poor sintering behavior are not suitable for use in the field of pulse energy storage alone. Therefore, the present invention selects Na 0.5 Bi 0.5 TiO3 is used as the base material, and then an equimolar high entropy ceramic (Bi 1 / 6 Na 1 / 6 Ca 1 / 6 Sr 1 / 6 Nd 1 / 6 Li 1 / 6 )TiO3 as dopant. Select high entropy ceramic (Bi1 / 6 Na 1 / 6 Ca 1 / 6 Sr 1 / 6 Nd 1 / 6 Li 1 / 6 )TiO3 for the following reasons: a. Its composition contains 6 elements at the A site, which destroy the long-range ordered ferroelectric domain structure and enhance the relaxation behavior due to different valence states and ionic radii; b. It includes a series of wide band gap oxides such as SrTiO3 (3.2eV), CaTiO3 (3.8eV) and Nd2O3 (5.05eV), which are high insulating additives when combined with Na 0.5 Bi 0.5 When TiO3 is doped, it can increase the impedance of the grains and reduce the impedance adaptation between the grains and the grain boundaries. This reduction in interface polarization can significantly increase E b value, thus obtaining an ultra-high density (18.2J / cm 3 ), high-performance lead-free ceramic material with high efficiency (85.6%) and high stability (20-120℃, 1-500Hz).
[0026] 2. The preparation method of the present invention is simple. Since the material preparation method adopts the traditional solid phase method, the reaction conditions are easy to control and have high repeatability. The equipment used is simple, easy to operate, low cost, and can be mass-produced, which has good industrialization prospects.
[0027] 3. All materials used in the present invention are lead-free materials, which are non-toxic and harmless to the environment and humans. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 (1-x)Na prepared in Example 1-5 of the present invention 0.5 Bi 0.5 TiO3-x(Bi 1 / 6 Na 1 / 6 Ca 1 / 6 Sr 1 / 6 Nd 1 / 6Li 1 / 6 ) X-ray spectrum of TiO3 material, where x is the number of moles, x=0, 0.25, 0.35, 0.45, 0.55;
[0029] Figure 2 (1-x)Na prepared in Example 5 of the present invention 0.5 Bi 0.5 TiO3-x(Bi 1 / 6 Na 1 / 6 Ca 1 / 6 Sr 1 / 6 Nd 1 / 6 Li 1 / 6) Microscopic morphology of TiO3 materials, where x is the molar number, x=0, 0.25, 0.35, 0.45, 0.55;
[0030] Figure 3 A single electrode loop diagram of a high energy storage density lead-free ceramic capacitor prepared in Example 6 of the present invention;
[0031] Figure 4 This is a high stability diagram of the high energy storage density lead-free ceramic capacitor prepared in Example 6 of the present invention. DETAILED DESCRIPTION
[0032] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0033] Example 1
[0034] A method for preparing a high energy storage density lead-free ceramic capacitor material comprises the following steps:
[0035] (1) Na2CO3 and Bi2O3TiO2 with analytical purity greater than 99% were mixed in a molar ratio of 0.5:0.5:1, ball-milled, dried, and pre-calcined to obtain Na 0.5 Bi 0.5 TiO3 powder, wherein the ball milling uses anhydrous ethanol as the medium and zirconia balls as the ball milling beads, the mixed ball milling is performed for 12 hours, the material is discharged using anhydrous ethanol, and the powder is dried at 70°C for 12 hours, and the powder is pre-calcined at a rate of 5°C / min to 850°C for 4 hours;
[0036] (2) Na2CO3, Bi2O3, CaCO3, SrCO3, Li2CO3, Nd2O3, and TiO2 of analytical purity greater than 99% were mixed in a molar ratio of 1 / 6:1 / 6:1 / 6:1 / 6:1 / 6:1 / 6:1, ball-milled, dried, and pre-calcined to obtain (Bi 1 / 6 Na 1 / 6 Ca 1 / 6 Sr 1 / 6 Nd 1 / 6 Li 1 / 6 ) TiO3 powder, wherein the ball milling uses anhydrous ethanol as the medium and zirconia balls as the ball milling beads, the mixed ball milling is performed for 12 hours, the material is discharged using anhydrous ethanol, and the material is dried at 70°C for 12 hours, and the material is pre-calcined at a rate of 5°C / min to 950°C for 4 hours;
[0037] (3) The pre-burned Na 0.5 Bi0.5 TiO3 powder and calcined (Bi 1 / 6 Na 1 / 6 Ca 1 / 6 Sr 1 / 6 Nd 1 / 6 Li 1 / 6 )TiO3 powder is prepared in a 1:0 molar ratio and ball milled, wherein the ball milling uses anhydrous ethanol as a medium and zirconia balls as ball milling beads, the mixture is ball milled for 12 hours, anhydrous ethanol is used to discharge the material, and the mixture is dried at 70°C for 12 hours. The high energy storage density lead-free ceramic capacitor material powder is obtained, and its nominal chemical formula is (1-x)Na 0.5 Bi 0.5 TiO3-x(Bi 1 / 6 Na 1 / 6 Ca 1 / 6 Sr 1 / 6 Nd 1 / 6 Li 1 / 6 )TiO3, where x=0.
[0038] Example 2
[0039] A method for preparing a high energy storage density lead-free ceramic capacitor material, which differs from Example 1 only in that: in the step (3), the pre-sintered Na 0.5 Bi 0.5 TiO3 powder and calcined (Bi 1 / 6 Na 1 / 6 Ca 1 / 6 Sr 1 / 6 Nd 1 / 6 Li 1 / 6 )TiO3 powder is mixed in a molar ratio of 0.75:0.25, and the nominal chemical formula of the high energy storage density lead-free ceramic capacitor material powder obtained is (1-x)Na 0.5 Bi 0.5 TiO3-x(Bi 1 / 6 Na 1 / 6 Ca 1 / 6 Sr 1 / 6 Nd 1 / 6 Li 1 / 6 )TiO3, where x=0.25.
[0040] Example 3
[0041] A method for preparing a high energy storage density lead-free ceramic capacitor material, which differs from Example 1 only in that: in the step (3), the pre-sintered Na 0.5 Bi 0.5 TiO3 powder and calcined (Bi 1 / 6 Na 1 / 6 Ca 1 / 6 Sr 1 / 6Nd 1 / 6 Li 1 / 6 )TiO3 powder is mixed in a molar ratio of 0.65:0.35, and the nominal chemical formula of the high energy storage density lead-free ceramic capacitor material powder obtained is (1-x)Na 0.5 Bi 0.5 TiO3-x(Bi 1 / 6 Na 1 / 6 Ca 1 / 6 Sr 1 / 6 Nd 1 / 6 Li 1 / 6 )TiO3, where x=0.35.
[0042] Example 4
[0043] A method for preparing a high energy storage density lead-free ceramic capacitor material, which differs from Example 1 only in that: in the step (3), the pre-sintered Na 0.5 Bi 0.5 TiO3 powder and calcined (Bi 1 / 6 Na 1 / 6 Ca 1 / 6 Sr 1 / 6 Nd 1 / 6 Li 1 / 6 )TiO3 powder is mixed in a molar ratio of 0.55:0.45, and the nominal chemical formula of the high energy storage density lead-free ceramic capacitor material powder obtained is (1-x)Na 0.5 Bi 0.5 TiO3-x(Bi 1 / 6 Na 1 / 6 Ca 1 / 6 Sr 1 / 6 Nd 1 / 6 Li 1 / 6 )TiO3, where x = 0.45.
[0044] Example 5
[0045] A method for preparing a high energy storage density lead-free ceramic capacitor material, which differs from Example 1 only in that: in the step (3), the pre-sintered Na 0.5 Bi 0.5 TiO3 powder and calcined (Bi 1 / 6 Na 1 / 6 Ca 1 / 6 Sr 1 / 6 Nd 1 / 6 Li 1 / 6 )TiO3 powder is mixed in a molar ratio of 0.45:0.55, and the nominal chemical formula of the high energy storage density lead-free ceramic capacitor material powder obtained is (1-x)Na 0.5 Bi 0.5 TiO3-x(Bi1 / 6 Na 1 / 6 Ca 1 / 6 Sr 1 / 6 Nd 1 / 6 Li 1 / 6 )TiO3, where x=0.55.
[0046] Table 1 Chemical composition of Examples 1-5
[0047] x-value chemical composition Example 1 0 <![CDATA[Na 0.5 Bi 0.5 TiO3]]> Example 2 0.25 <![CDATA[0.75Na 0.5 The 0.5 TiO3–0.25(Bi 1 / 6 And 1 / 6 Ca 1 / 6 Sr 1 / 6 Nd 1 / 6 Li 1 / 6 )TiO3]]> Example 3 0.35 <![CDATA[0.65Na 0.5 The 0.5 TiO3–0.35(Bi 1 / 6 And 1 / 6 Ca 1 / 6 Sr 1 / 6 Nd 1 / 6 Li 1 / 6 )TiO3]]> Example 4 0.45 <![CDATA[0.55Na 0.5 The 0.5 TiO3–0.45(Bi 1 / 6 And 1 / 6 Ca 1 / 6 Sr 1 / 6 Nd 1 / 6 Li 1 / 6 )TiO3]]> Example 5 0.55 <![CDATA[0.45Na 0.5 The 0.5 TiO3–0.55(Bi 1 / 6 And 1 / 6 Ca 1 / 6 Sr 1 / 6 Nd 1 / 6 Li 1 / 6 )TiO3]]>
[0048] Figure 1 The XRD patterns of the ceramics prepared in Examples 1 to 5 are shown. The results show that the ceramics prepared in Examples 1 to 5 are all pure perovskite structures without any second phase, and are pseudo cubic phase structures.
[0049] Figure 2 Shown is a scanning electron microscope image of the ceramic prepared in Example 5. The results show that the samples all have clear grain morphology and a microstructure with uniform grain size and compactness.
[0050] Example 6
[0051] A method for preparing a high energy storage density lead-free ceramic capacitor comprises the following steps:
[0052] (1) The high energy storage density lead-free ceramic capacitor material powders prepared in Examples 1-5 were respectively added with a polyvinyl alcohol aqueous solution binder having a content of 0.65 mL / g relative to the powder for granulation, and tableted in a mold with a diameter of 10 mm to obtain a circular ceramic body;
[0053] (2) heating the prepared circular ceramic body to 600° C. and keeping the temperature for 6 h to perform binder removal;
[0054] (3) calcining the debinding circular ceramic body at 1200° C. for 4 h to obtain a lead-free ceramic with high energy storage density;
[0055] (4) The surface of the high energy storage density lead-free ceramic was polished with 5000-grit sandpaper and ultrasonically cleaned with alcohol. Then, an ion sputtering device was used to spray gold on the polished sample surface. The current was sputtered for 80 seconds at an intensity of 5 mA to obtain a high energy storage density lead-free ceramic capacitor.
[0056] Figure 3 The single-stage hysteresis loop of the lead-free ceramic capacitor prepared by the high energy storage density lead-free ceramic capacitor material of Examples 1-5 under the breakdown electric field is shown. The results show that as the high entropy ceramic (Bi 1 / 6 Na 1 / 6 Ca 1 / 6 Sr 1 / 6 Nd 1 / 6Li1 / 6 ) With the increase of TiO3 content, the breakdown electric field gradually increases, and the single-stage hysteresis loop becomes more slender, which indicates that the introduction of high entropy enhances the relaxation behavior. Finally, at 0.45Na 0.5 Bi 0.5 TiO3-0.55(Bi 1 / 6 Na 1 / 6 Ca 1 / 6 Sr 1 / 6 Nd 1 / 6 Li 1 / 6 )TiO3 ceramic capacitors have been obtained with ultra-high density (18.2J / cm 3 ), high efficiency (85.6%) and excellent performance.
[0057] Figure 4 The results are shown using 0.45Na 0.5 Bi 0.5 TiO3-0.55(Bi 1 / 6 Na 1 / 6 Ca 1 / 6 Sr 1 / 6 Nd 1 / 6Li 1 / 6 )TiO3 prepared lead-free ceramic capacitor under 200kV / cm electric field variable temperature and frequency single-stage hysteresis loop, the results show that the ceramic capacitor has the characteristics of high stability (20-120℃, 1-500Hz).
[0058] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the structure of the present invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. A high energy storage density lead-free ceramic capacitor material, Features: According to (1-x)(Na 0.5 Bi 0.5 TiO 3 )-x(Bi 1 / 6 Na 1 / 6 Ca 1 / 6 Sr 1 / 6 Nd 1 / 6 Li 1 / 6 )TiO 3 The stoichiometric ratio is used, wherein x is the number of moles, and the value range of x is 0≤x≤0.
55.
2. A method for preparing a lead-free ceramic capacitor material with high energy storage density according to claim 1, It is characterized in that The following steps are involved: (1) Put Na 2 CO 3 、Bi 2 O 3 、TiO 2 Mixing, ball milling, drying, and pre-calcining to obtain Na 0.5 Bi 0.5 TiO 3 Powder; (2) Put Na 2 CO 3 、Bi 2 O 3 、CaCO 3 、SrCO 3 , Li 2 CO 3 、Nd 2 O 3 、TiO 2 Mixing, ball milling, drying, and pre-calcining to obtain (Bi 1 / 6 Na 1 / 6 Ca 1 / 6 Sr 1 / 6 Nd 1 / 6 Li 1 / 6 )TiO 3 Powder; (3) Put Na 0.5 Bi 0.5 TiO 3 Powder and (Bi 1 / 6 Na 1 / 6 Ca 1 / 6 Sr 1 / 6 Nd 1 / 6 Li 1 / 6 )TiO 3 The powders are mixed, ball-milled and dried to obtain the lead-free ceramic capacitor material with high energy storage density.
3. The method for preparing a lead-free ceramic capacitor material with high energy storage density according to claim 2, Features: In the step (1), Na 2 CO 3 、Bi 2 O 3 、TiO 2 The molar ratio is 0.5:0.5:1, the pre-calcination temperature is 800-900°C, the pre-calcination time is 3-6h, and the heating rate is 3-5°C / min.
4. The method for preparing a lead-free ceramic capacitor material with high energy storage density according to claim 2, Features: In the step (1), Na 2 CO 3 、Bi 2 O 3 、CaCO 3 、SrCO 3 , Li 2 CO 3 、Nd 2 O 3 、TiO 2 The molar ratio is 1 / 6:1 / 6:1 / 6:1 / 6:1 / 6:1 / 6:1 / 6:1, the pre-sintering temperature is 900-1000°C, the pre-sintering time is 3-6h, and the heating rate is 3-5°C / min.
5. The method for preparing a lead-free ceramic capacitor material with high energy storage density according to claim 2, Features: The ball milling process uses anhydrous ethanol as the medium and zirconium oxide balls as the ball milling beads. The mixed ball milling process is performed for 10-12 hours. Anhydrous ethanol is used for discharging. The drying temperature is 60-80° C. and the drying time is 10-12 hours.
6. A method for preparing a lead-free ceramic capacitor with high energy storage density, It is characterized in that The following steps are involved: (1) Adding a binder to the high energy storage density lead-free ceramic capacitor material of claim 1 to granulate the material, and pressing the material into tablets to obtain a circular ceramic body; (2) heating the round ceramic body to remove binder; (3) calcining the round ceramic body after debinding to obtain lead-free ceramic; (4) The lead-free ceramic surface is polished and cleaned, and then a gold electrode is sprayed on the surface to obtain the high energy storage density lead-free ceramic capacitor.
7. The method for preparing a lead-free ceramic capacitor with high energy storage density according to claim 6, Features: In the step (1), the adhesive is a 4wt%-6wt% aqueous solution of polyvinyl alcohol, and the tableting is carried out in a mold with a diameter of 8-12 mm.
8. The method for preparing a lead-free ceramic capacitor with high energy storage density according to claim 6, Features: In the step (2), the ceramic plastic body is heated for debinding at a temperature of 500-700° C. and the heat preservation time is 5-7 hours.
9. The method for preparing a lead-free ceramic capacitor with high energy storage density according to claim 6, Features: In the step (3), the calcination temperature is 1150-1250° C. and the calcination time is 3-6 hours.
10. The method for preparing a lead-free ceramic capacitor with high energy storage density according to claim 6, Features: In the step (4), 2000-10000 mesh sandpaper is used for polishing, and an ion sputtering device is used for gold spraying, and the gold spraying time is 60-120 seconds.
Citation Information
Patent Citations
B-bit local high-entropy ceramic material with nano polarization structure, and preparation method and application thereof
CN113620703A
Sodium bismuth titanate-based high-entropy ceramic material with high energy storage characteristic as well as preparation method and application of sodium bismuth titanate-based high-entropy ceramic material
CN116082034A
Sodium bismuth titanate-based high-entropy dielectric energy storage ceramic material as well as preparation method and application thereof
CN116854469A
Sodium bismuth titanate-based high-entropy energy storage ceramic material and preparation method thereof
CN117735976A