Microporous ceramic catalyst carrier and preparation method thereof

By using bauxite and other components to prepare microporous ceramic catalyst support, the problem of low strength of alumina support is solved, the high strength and wear resistance of the support are achieved, the complex reaction design is adapted, and the stability of the support is ensured. Non-polluting.

CN118930311AActive Publication Date: 2024-11-12YUAN QIU XIN CAI LIAO (NAN TONG) YOU XIAN GONG SI
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202411148188.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-12
Estimated Expiration
2044-08-21

AI Technical Summary

Technical Problem

The existing microporous ceramic catalyst support uses alumina as the raw material, which is low in strength and easy to damage, resulting in deviations during reaction.

Method used

Bauxite is used as the main base material, combined with fused silica and porcelain clay, and heat-resistant phenolic resin, methyl hydroxypropyl cellulose, polyvinyl alcohol, sodium silicate, sodium dodecyl sulfate, magnesium oxide, and active oxidation. Components such as zinc, denitrification catalyst and amorphous silicon carbide catalyst are prepared by sintering and glaze coating to improve the strength and wear resistance of the carrier.

Benefits of technology

The prepared microporous ceramic catalyst support has low density, high strength, strong compressive resistance, stable chemical properties, adapts to complex reaction designs, and is pollution-free, and is suitable for assembly in various shapes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930311A_ABST
    Figure CN118930311A_ABST
Patent Text Reader

Abstract

The invention discloses a microporous ceramic catalyst carrier and a preparation method thereof, and relates to the technical field. The base material is prepared from the following components in parts by weight: 30 to 50 parts of bauxite, 47 to 60 parts of fused quartz and 10 to 36 parts of porcelain clay; the adhesive is prepared from the following components in parts by weight: 10 to 14 parts of heat-resistant phenolic resin, 23 to 26 parts of fumed silica and 10 to 16 parts of mica powder. According to the microporous ceramic catalyst carrier, the bauxite is used as a main base material to replace aluminum oxide, and the bauxite internally contains silicon oxide with low content, so that the bauxite can be better fused with fused quartz during sintering to reduce the sintering temperature, improve the molding rate and enhance the wear resistance, and after the microporous ceramic catalyst carrier is molded, the service life of the microporous ceramic catalyst carrier is prolonged. The composite material has the advantages of low density, high strength, compression resistance, stable chemical property, high universality, no pollution, capability of being assembled in various shapes and adaptability to complex reaction design.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field, and in particular to a microporous ceramic catalyst carrier and a preparation method thereof. Background Art

[0002] Catalyst immobilization technology is an important means to make enzyme catalysis more widely and effectively utilized. It requires the following three aspects of work to complete: (1) extraction and purification of raw enzymes; (2) preparation of carriers; (3) immobilization of enzymes. At present, the research on enzyme purification technology and immobilization methods has been relatively developed. The success of immobilized enzymes mostly relies on the performance of the carrier to design and synthesize carriers with excellent and controllable performance. Microporous ceramics are a kind of functional structural ceramics. The interior or surface of the ceramic body contains a large number of open or closed micropores with a pore size of micrometer or submicrometer. This porous solid surface characteristic makes it have a large internal surface, that is, a large surface energy, and thus has a strong adsorption capacity, which is suitable as a carrier.

[0003] In the prior art, alumina is used as a raw material in microporous ceramic catalyst carriers. The microporous ceramic catalyst carriers made of alumina have low strength and are easily damaged during use, which leads to deviations during the reaction.

[0004] Therefore, the present invention proposes a microporous ceramic catalyst carrier and a preparation method thereof to solve this problem. Summary of the invention

[0005] The purpose of this application is to solve the problems in the above-mentioned background technology. This application provides a microporous ceramic catalyst carrier and a preparation method thereof.

[0006] In order to achieve the above-mentioned purpose, this application specifically adopts the following technical solutions: A microporous ceramic catalyst carrier comprises the following raw materials: A base material, the base material comprising the following components in parts by weight: 30-50 parts of bauxite, 47-60 parts of fused quartz, and 10-36 parts of porcelain clay; Adhesive, the adhesive comprises the following components in parts by weight: 10-14 parts of heat-resistant phenolic resin, 23-26 parts of fumed silica, and 10-16 parts of mica powder; A reinforcing agent, the component of which is 15-17 parts, and the reinforcing agent acts on the adhesive to increase the connection strength between the adhesive and the base material; The raw materials also include the following components: 6-17 parts of dispersant, 16-24 parts of glaze, 25-27 parts of catalyst and 30-33 parts of dehydration component; Bauxite is used as the main base material to replace alumina. Since it also contains silicon oxide and the content is not high, it can be better fused with molten quartz during sintering, which is used to reduce the sintering temperature, increase the forming rate and enhance the wear resistance. As a result, when the microporous ceramic catalyst carrier is formed, it has the advantages of low density, high strength, compression resistance, stable chemical properties, strong universality, no pollution, can be assembled in various shapes, and adapt to complex reaction designs.

[0007] Further, the heat-resistant phenolic resin is a boron phenolic resin, and its weight parts are 12 parts; Boron phenolic resin is used as a raw material. Firstly, the raw material of boron phenolic resin is easy to obtain and the preparation cost is low. Secondly, the boron phenolic resin is an epoxy-modified boron phenolic resin. The phenolic hydroxyl group in the phenolic resin and the hydroxyl group in the bisphenol A epoxy resin undergo an etherification reaction, so that the hydroxyl group in the phenolic resin and the hydroxyl group in the bisphenol A epoxy resin are combined with each other, and a molecule of water is removed to form an ether bond. Then, the hydroxymethyl in the phenolic resin and the epoxy group at the end of the bisphenol A epoxy resin undergo a ring-opening reaction to form a three-dimensional structure. It can also be said that the curing effect of the bisphenol A epoxy resin is stimulated by the phenolic resin, and the structure changes further. Due to its complex structure, the modified resin has good adhesion and toughness.

[0008] Further, the reinforcing agent comprises the following components in parts by weight: 8 parts of methyl hydroxypropyl cellulose and 8 parts of polyvinyl alcohol; By arranging methyl hydroxypropyl cellulose and polyvinyl alcohol, methyl hydroxypropyl cellulose imparts lubricity and water retention between the raw material components during the reaction, and improves the original strength of the raw material. The concentrated solution is adsorbed on the surface of the ceramic particles, which reduces the friction between the particles and enhances their lubricity, further increasing the strength of the microporous ceramic catalyst carrier after molding. Polyvinyl alcohol is a polymer compound that is bonded through hydrogen bonding, hydroxyl reaction, sodium ion action and cross-linking structure, and is used to increase the connection strength between the various components in the raw material.

[0009] Further, the dispersant includes the following components in parts by weight: 8 parts of sodium silicate, 2 parts of sodium dodecyl sulfate, and 4 parts of methyl amyl alcohol; Sodium silicate, sodium dodecyl sulfate and methyl amyl alcohol are used as dispersants. When used, the main mechanism of sodium silicate as a dispersant is the interaction of multiple factors such as its ionic properties, hydrate formation, surface activity and alkalinity, which enables it to be effectively dispersed in water. The dodecyl chain in the molecular structure of sodium dodecyl sulfate is hydrophobic, while sulfate and sodium ions are hydrophilic. When sodium dodecyl sulfate is dissolved in water, it can form a micellar structure with a hydrophilic head group having a hydrophobic chain. This structure enables sodium dodecyl sulfate to reduce the surface tension of the liquid surface and has emulsifying and dispersing effects. Methyl amyl alcohol forms an adsorption layer on the surface of solid particles, which increases the charge on the surface of the solid particles and increases the reaction force between particles that forms steric hindrance.

[0010] Further, the glaze comprises the following components in parts by weight: 10 parts of magnesium oxide, 4 parts of sodium chloride, and 3 parts of active zinc oxide; When in use, sodium chloride and active zinc oxide are initially fused using magnesium oxide as a solvent to form a glaze, which acts as a protective paint and adheres to the surface of the microporous ceramic catalyst carrier, reducing the possibility of wear on the microporous ceramic catalyst carrier by external objects.

[0011] Furthermore, the catalyst comprises the following components in parts by weight: 12 parts of denitration catalyst and 14 parts of amorphous silicon carbide catalyst.

[0012] Further, the dehydration component includes the following components in parts by weight: 15 parts of activated carbon, 17 parts of sponge; When in use, the activated carbon is applied to the outside of the porcelain clay and bauxite, and then wrapped on the outside with a sponge, thereby absorbing the moisture inside the two, reducing excess moisture and reducing the impact on the concentration of other raw materials.

[0013] Furthermore, the components of the raw materials are 43 parts of bauxite, 55 parts of fused quartz, 27 parts of porcelain clay, 12 parts of heat-resistant phenolic resin, 24 parts of fumed silica, 16 parts of mica powder, 16 parts of reinforcing agent, 14 parts of dispersant, 17 parts of glaze, 26 parts of catalyst, and 32 parts of dehydration component.

[0014] The present application also provides a method for preparing a microporous ceramic catalyst carrier, which is used to prepare the above-mentioned microporous ceramic catalyst carrier, comprising the following steps: S1, mixing the dehydrated component with the base material, and dehydrating the base material; S2, selecting a base material and an adhesive and mixing the two to obtain a first material; S3, adding a reinforcing agent, a dispersant and a catalyst to the first expectation and mixing them to obtain a second expectation; S4, drying, shaping and firing the second material to obtain a body, and applying glaze on the body to complete the preparation.

[0015] Furthermore, in the step S4, when the embryo is shaped, it is set into a cylindrical shape, and when the glaze is applied, the radial ends of the cylindrical embryo are applied.

[0016] The beneficial effects of this application are as follows: The present application uses bauxite as the main base material to replace alumina. Since it also contains silicon oxide and the content is not high, it can be better fused with molten quartz during sintering, which is used to reduce the sintering temperature, increase the forming rate and enhance the wear resistance. As a result, when the microporous ceramic catalyst carrier is formed, it has the advantages of low density, high strength, compression resistance, stable chemical properties, strong universality, no pollution, can be assembled in various shapes, and adapt to complex reaction designs.

[0017] The present application uses boron phenolic resin as a raw material. Firstly, the raw material of boron phenolic resin is easy to obtain and the preparation cost is low. Secondly, the boron phenolic resin is an epoxy-modified boron phenolic resin. The phenolic hydroxyl groups in the phenolic resin and the hydroxyl groups in the bisphenol A epoxy resin undergo an etherification reaction, so that the hydroxyl groups in the phenolic resin and the hydroxyl groups in the bisphenol A epoxy resin are combined with each other, and a molecule of water is removed to form an ether bond. Then, the hydroxymethyl groups in the phenolic resin and the epoxy groups at the ends of the bisphenol A epoxy resin undergo a ring-opening reaction to form a three-dimensional structure. It can also be said that the curing effect of the bisphenol A epoxy resin is stimulated by the phenolic resin, and the structure further changes. Due to its complex structure, the modified resin has good adhesion and toughness.

[0018] The present application is provided with methyl hydroxypropyl cellulose and polyvinyl alcohol. During the reaction, the methyl hydroxypropyl cellulose imparts lubricity and water retention to the raw material components and improves the original strength of the raw material. The concentrated solution is adsorbed on the surface of the ceramic particles, which reduces the friction between the particles and enhances their lubricity, further increasing the strength of the microporous ceramic catalyst carrier after molding. Polyvinyl alcohol is a polymer compound that is bonded by hydrogen bonding, hydroxyl reaction, sodium ion action and cross-linking structure, and is used to increase the connection strength between the components in the raw material.

[0019] The present application uses sodium silicate, sodium dodecyl sulfate and methyl amyl alcohol as dispersants. When used, the main mechanism of sodium silicate as a dispersant is the interaction of multiple factors such as its ionic properties, hydrate formation, surface activity and alkalinity, which enables it to be effectively dispersed in water. The dodecyl chain in the molecular structure of sodium dodecyl sulfate is hydrophobic, while the sulfate group and sodium ion are hydrophilic. When sodium dodecyl sulfate is dissolved in water, it can form a micellar structure with a hydrophilic head group having a hydrophobic chain. This structure enables sodium dodecyl sulfate to reduce the surface tension of the liquid surface and has emulsifying and dispersing effects. Methyl amyl alcohol forms an adsorption layer on the surface of solid particles, which increases the charge on the surface of the solid particles and improves the reaction force between particles that forms steric hindrance.

[0020] When the present application is used, magnesium oxide is used as a solvent to initially fuse sodium chloride and active zinc oxide to form a glaze, which acts as a protective paint and adheres to the surface of the microporous ceramic catalyst carrier, reducing the possibility of wear of the microporous ceramic catalyst carrier by external objects.

[0021] The present application uses a denitration catalyst and an amorphous silicon carbide catalyst as catalysts. When in use, the denitration catalyst can play a catalytic role. At the same time, the denitration catalyst reduces the nitrogen oxide content in the exhaust gas by converting nitrogen oxides into nitrogen and water vapor, thereby achieving the purpose of reducing air pollution. The principle of the SCR denitration process is that under the action of the catalyst, the reducing agent reacts with the nitrogen oxides in the flue gas to generate harmless nitrogen and water, thereby removing the nitrogen oxides in the flue gas. The amorphous silicon carbide catalyst has high catalytic activity and thermal stability. The substrate molecules undergo physical adsorption or chemical adsorption with the ASC catalyst surface through the carbon-silicon bond on the active site, so that the substrate molecules undergo a chemical reaction on the catalyst surface to form an active intermediate. The active intermediate further reacts to generate a product, and the product is desorbed from the catalyst surface to release the catalyst to re-participate in the reaction.

[0022] When the present application is used, the activated carbon is applied to the outside of the porcelain clay and bauxite, and then wrapped on the outside with a sponge, thereby absorbing the moisture inside the two, reducing excess moisture and reducing the impact on the concentration of other raw materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 It is a schematic diagram of the preparation process steps of this application. DETAILED DESCRIPTION

[0024] In order to make the purpose, technical solutions and advantages of the embodiments of the present application clearer, the technical solutions in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application.

[0025] A microporous ceramic catalyst carrier provided in one embodiment of the present application includes the following raw materials: The base material includes the following components by weight: 30-50 parts of bauxite, which contains not only aluminum oxide but also silicon oxide. Kaolin can also be added to the raw material. The preparation using bauxite as the raw material also solves the problem of using inferior mineral resources, has strong scalability, and solves the problem of low universality of catalyst carriers; 47-60 parts of fused quartz. Fused quartz is made by melting natural high-purity silicon dioxide in an electric furnace at a temperature above 1760°C and then rapidly cooling it. This process converts crystalline silicon dioxide into amorphous glass melt. The melting temperature of fused quartz is about 1713°C, and its thermal conductivity is low. Its thermal expansion coefficient is almost the smallest among all refractory materials. Therefore, it has extremely high thermal shock stability. During the reaction, it is easy to combine bauxite with fused quartz through the silicon oxide in bauxite. As a result, after the microporous ceramic catalyst carrier is formed, it has the advantages of low density, high strength, pressure resistance, stable chemical properties, strong universality, no pollution, and can be assembled in various shapes to adapt to complex reaction designs. 10-36 parts of porcelain clay, as the basic material for preparing ceramics, plays the role of basic aggregate during sintering and is used to carry other raw materials; The adhesive comprises the following components in parts by weight: 10-14 parts of heat-resistant phenolic resin, which can also act as a filler. When used, after the heat-resistant phenolic resin is melted, it is convenient to bond the remaining parts in the raw material, and it has the advantages of high temperature resistance, oxidation resistance, erosion resistance, high mechanical strength, etc. The use temperature in an oxidizing environment can reach more than 1000°C, which further increases the strength and heat resistance of the microporous ceramic catalyst carrier; 23-26 parts of fumed silica. Fumed silica can also replace nano-alumina. Since there are fewer aluminum ions in bauxite, it can replace aluminum ions, so that less aluminum ions can also make ceramics form. It can play the role of nanoparticles. At the same time, it is a gas-phase particle, which not only improves the strength and toughness of ceramic materials, but also improves the hardness and elastic modulus of materials. Its effect is more ideal than adding alumina. Using fumed silica to composite ceramic substrates not only improves the density, toughness and smoothness of the device after forming, but also greatly reduces the sintering temperature; 10-16 parts of mica powder, which also contains some alumina to supplement aluminum ions, and has good wear resistance. The mica powder also has plasticity and flexibility, which is convenient for shaping the microporous ceramic catalyst carrier after it is prepared. A reinforcing agent, the component of the reinforcing agent is 15-17 parts, and the reinforcing agent acts on the adhesive to increase the connection strength between the adhesive and the base material. When used, the reinforcing agent increases the effect of the adhesive, thereby increasing the degree of fusion between the base materials, thereby facilitating the molding of the microporous ceramic catalyst carrier; The raw materials also include the following components: 6-17 parts of dispersant, which is used to disperse the tension of the liquid surface after the various materials are melted, so as to facilitate better fusion between the materials; 16-24 parts of glaze. After the microporous ceramic catalyst carrier is formed, the microporous ceramic catalyst carrier is protected by applying glaze to reduce friction during transportation or when not in use. 25-27 parts of a catalyst, the catalyst is used to increase the reaction rate, thereby improving the preparation efficiency; 30-33 parts of dehydration components, before preparation, the porcelain clay and bauxite are dehydrated by the dehydration components to remove excess water, thereby reducing the influence of excess water on the subsequent raw material concentration and increasing the feasibility of the reaction; Compared with the prior art, bauxite is used as the main base material to replace alumina. Since it also contains silicon oxide and the content is not high, it can be better fused with molten quartz during sintering, which is used to reduce the sintering temperature, increase the forming rate and enhance the wear resistance. As a result, after the microporous ceramic catalyst carrier is formed, it has the advantages of low density, high strength, compression resistance, stable chemical properties, strong universality, no pollution, can be assembled in various shapes, and adapt to complex reaction designs.

[0026] In some embodiments, the heat-resistant phenolic resin is a boron phenolic resin, and its weight proportion is 12 parts. First, the raw materials of the boron phenolic resin are easily available and the preparation cost is relatively low. Second, the boron phenolic resin is an epoxy-modified boron phenolic resin. The phenolic hydroxyl groups in the phenolic resin and the hydroxyl groups in the bisphenol A epoxy resin undergo an etherification reaction, so that the hydroxyl groups in the phenolic resin and the hydroxyl groups in the bisphenol A epoxy resin are combined with each other, and a molecule of water is removed to form an ether bond. After that, the hydroxymethyl groups in the phenolic resin and the epoxy groups at the ends of the bisphenol A epoxy resin undergo a ring-opening reaction to form a three-dimensional structure. It can also be said that the curing effect of the bisphenol A epoxy resin is stimulated by the phenolic resin, and the structure further changes. Due to its complex structure, the modified resin will have good adhesion and toughness.

[0027] In some embodiments, the reinforcing agent includes the following components in parts by weight: 8 parts of methyl hydroxypropyl cellulose, which imparts lubricity and water retention between the raw material components and improves the original strength of the raw material. The concentrated solution is adsorbed on the surface of the ceramic particles, which reduces the friction between the particles and enhances their lubricity, further increasing the strength of the microporous ceramic catalyst carrier after molding; 8 parts of polyvinyl alcohol. Polyvinyl alcohol is a high molecular compound that is bonded through hydrogen bonding, hydroxyl reaction, sodium ion action and cross-linking structure, and is used to increase the connection strength between the various components in the raw materials.

[0028] In some embodiments, the dispersant includes the following components in parts by weight: 8 parts of sodium silicate, the main mechanism of sodium silicate as a dispersant is through the interaction of multiple factors such as its ionic properties, hydrate formation, surface activity and alkalinity, which enables it to be effectively dispersed in water; 2 parts of sodium dodecyl sulfate. The dodecyl chain in its molecular structure is hydrophobic, while the sulfate and sodium ions are hydrophilic. When sodium dodecyl sulfate is dissolved in water, it can form a micellar structure with a hydrophilic head group having a hydrophobic chain. This structure enables sodium dodecyl sulfate to reduce the surface tension of the liquid surface and has emulsifying and dispersing effects; 4 parts of methylpentanol forms an adsorption layer on the surface of the solid particles, increases the charge on the surface of the solid particles, and enhances the reaction force between the particles to form steric hindrance.

[0029] In some embodiments, the glaze includes the following components in parts by weight: 10 parts of magnesium oxide, 4 parts of sodium chloride, and 3 parts of active zinc oxide. When used, sodium chloride and active zinc oxide are initially fused using magnesium oxide as a solvent to form a glaze, which acts as a protective paint and adheres to the surface of the microporous ceramic catalyst carrier, thereby reducing the possibility of wear on the microporous ceramic catalyst carrier by external objects.

[0030] In some embodiments, the catalyst includes the following components in parts by weight: 12 parts of a denitration catalyst, which can play a catalytic role while reducing the nitrogen oxide content in the exhaust gas by converting nitrogen oxides into nitrogen and water vapor, thereby achieving the purpose of reducing air pollution. The principle of the SCR denitration process is that under the action of the catalyst, the reducing agent reacts with the nitrogen oxides in the flue gas to generate harmless nitrogen and water, thereby removing the nitrogen oxides in the flue gas; 14 parts of amorphous silicon carbide catalyst, which has high catalytic activity and thermal stability. The substrate molecules undergo physical or chemical adsorption on the surface of the ASC catalyst through the carbon-silicon bonds on the active sites, so that the substrate molecules undergo chemical reactions on the catalyst surface to form active intermediates. The active intermediates further react to generate products, which are desorbed from the catalyst surface, releasing the catalyst to re-participate in the reaction.

[0031] In some embodiments, the dehydration component includes the following components in parts by weight: 15 parts of activated carbon and 17 parts of sponge. When in use, the activated carbon is applied to the outside of the porcelain clay and bauxite, and then wrapped on the outside with a sponge to absorb the moisture inside the two, thereby reducing excess moisture and reducing the impact on the concentration of other raw materials.

[0032] In some embodiments, the raw material components are 43 parts of bauxite, 55 parts of fused quartz, 27 parts of china clay, 12 parts of heat-resistant phenolic resin, 24 parts of fumed silica, and 16 parts of mica powder; 16 parts of reinforcing agent, including 8 parts of methyl hydroxypropyl cellulose and 8 parts of polyvinyl alcohol; 14 parts of dispersant, including 8 parts of sodium silicate, 2 parts of sodium lauryl sulfate, and 4 parts of methyl amyl alcohol; 17 parts of glaze, including 10 parts of magnesium oxide, 4 parts of sodium chloride, and 3 parts of active zinc oxide; 26 parts of catalyst, including 12 parts of denitration catalyst and 14 parts of amorphous silicon carbide catalyst; 32 parts of dehydrated components, including 15 parts of activated carbon and 17 parts of sponge; During preparation, each component is weighed in batches to facilitate subsequent preparation.

[0033] like Figure 1 As shown, the present application also provides a method for preparing a microporous ceramic catalyst carrier, which is used to prepare the above-mentioned microporous ceramic catalyst carrier, comprising the following steps: S1. Mixing the dehydrated component with the base material to dehydrate the base material. When in use, wrapping the dehydrated component on the outside of the base material to absorb the moisture inside the base material; S2, selecting a base material and an adhesive and mixing the two to obtain a first material; S3, adding a reinforcing agent, a dispersant and a catalyst to the first expectation and mixing them to obtain a second expectation; S4, drying, shaping and firing the second material to obtain a body, and applying glaze on the body to complete the preparation.

[0034] like Figure 1 As shown, in some embodiments, in step S4, when the embryo is shaped, it is set into a cylindrical shape, and when the glaze is applied, the radial ends of the cylindrical embryo are applied. When in use, the glaze is applied to the ends of the cylindrical embryo, so that when it is stored, its bottom is protected by the glaze and its column body is exposed to the outside, which is convenient for it to better contact with the reactants when used, thereby increasing the practicality of the microporous ceramic catalyst carrier.

[0035] The above description of the disclosed embodiments enables those skilled in the art to implement or use the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A microporous ceramic catalyst carrier, characterized in that: The ingredients include: A base material, the base material comprising the following components in parts by weight: 30-50 parts of bauxite, 47-60 parts of fused quartz, and 10-36 parts of porcelain clay; Adhesive, the adhesive comprises the following components in parts by weight: 10-14 parts of heat-resistant phenolic resin, 23-26 parts of fumed silica, and 10-16 parts of mica powder; A reinforcing agent, the component of which is 15-17 parts, and the reinforcing agent acts on the adhesive to increase the connection strength between the adhesive and the base material; The raw materials also include the following components: 6-17 parts of dispersant, 16-24 parts of glaze, 25-27 parts of catalyst and 30-33 parts of dehydration component.

2. The microporous ceramic catalyst carrier according to claim 1, characterized in that: The heat-resistant phenolic resin is boron phenolic resin, and its weight part is 12 parts.

3. The microporous ceramic catalyst carrier according to claim 1, characterized in that: The reinforcing agent comprises the following components in parts by weight: 8 parts of methyl hydroxypropyl cellulose and 8 parts of polyvinyl alcohol.

4. The microporous ceramic catalyst carrier according to claim 1, characterized in that: The dispersant includes the following components in parts by weight: 8 parts of sodium silicate, 2 parts of sodium dodecyl sulfate, and 4 parts of methyl amyl alcohol.

5. The microporous ceramic catalyst carrier according to claim 1, characterized in that: The glaze comprises the following components in parts by weight: 10 parts of magnesium oxide, 4 parts of sodium chloride, and 3 parts of active zinc oxide.

6. The microporous ceramic catalyst carrier according to claim 1, characterized in that: The catalyst comprises the following components in parts by weight: 12 parts of a denitration catalyst and 14 parts of an amorphous silicon carbide catalyst.

7. The microporous ceramic catalyst carrier according to claim 1, characterized in that: The dehydration component includes the following components in parts by weight: 15 parts of activated carbon and 17 parts of sponge.

8. The microporous ceramic catalyst carrier according to claim 1, characterized in that: The components of the raw materials are 43 parts of bauxite, 55 parts of fused quartz, 27 parts of porcelain clay, 12 parts of heat-resistant phenolic resin, 24 parts of fumed silica, 16 parts of mica powder, 16 parts of reinforcing agent, 14 parts of dispersant, 17 parts of glaze, 26 parts of catalyst and 32 parts of dehydrating component.

9. A method for preparing a microporous ceramic catalyst carrier, used for preparing the microporous ceramic catalyst carrier according to any one of claims 1 to 8, characterized in that: The following steps are involved: S1, mixing the dehydrated component with the base material, and dehydrating the base material; S2, selecting a base material and an adhesive and mixing the two to obtain a first material; S3, adding a reinforcing agent, a dispersant and a catalyst to the first expectation and mixing them to obtain a second expectation; S4, drying, shaping and firing the second material to obtain a body, and applying glaze on the body to complete the preparation.

10. The method for preparing a microporous ceramic catalyst carrier according to claim 9, characterized in that: In the step S4, when the embryo is shaped, it is set into a cylindrical shape, and when the glaze is applied, the radial ends of the cylindrical embryo are applied.

Citation Information

Patent Citations

  • Porous ceramic bodies and process for their preparation

    CN101795996A

  • Microporous ceramic catalyst carrier and preparation method thereof

    CN105396624A

  • Low-shrinkage high-strength porous ceramic, preparation method and atomizing core

    CN117534450A

  • Thin wall cordierite carrier for ceramic honeycomb catalyst and method for preparing the same

    CN1827217A

  • Cordierite honeycomb structural body and method of producing the same

    EP0227482A2