Ultrathin Al2O3 ceramic substrate metallization copper cladding and densification process
Through copper oxide sintering reduction and pulse plating technology, the high cost and process complexity problems in the metallization process of ultra-thin Al2O3 ceramic substrates are solved, and high-quality and dense copper layer adhesion is achieved, which improves the bonding strength and performance of the copper layer. .
Patent Information
- Application Number
- CN202411103386.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-11-12
AI Technical Summary
The existing metallization process of ultra-thin Al2O3 ceramic substrates has high cost, complex process, low bond strength of copper layer, easy oxidation and uneven quality, making it difficult to achieve low cost, simple process, dense copper layer and high bond strength. deal with.
Using copper oxide sintering, reducing metallization and pulse plating densification, high-quality metal copper is formed by ultrasonic cleaning, organic carrier modulation of CuO slurry, coating or screen printing, glue discharge sintering, reduction treatment and pulse plating technology. layer.
Metalization of ultra-thin ceramic substrates with low cost, simple process, dense copper layer, high bond strength, and difficult to oxidize is achieved, filling the gaps in the prior art and improving the density and quality of the copper layer.
Smart Images

Figure CN118930323A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of ceramic substrate metallization, and in particular relates to a method for metallizing the surface of an ultra-thin Al2O3 ceramic substrate and a method for densifying a porous copper layer by pulse electroplating. Background Art
[0002] Ultra-thin Al2O3 ceramic substrates are used for metallization copper plating research. On the one hand, Al2O3 is cost-effective and is a mature ceramic substrate. On the other hand, its ultra-thin characteristics can improve the heat dissipation performance of the ceramic substrate, reduce the weight, and have the advantages of miniaturization and lightweight. Metallization and subsequent pulse electroplating copper layer densification treatment on ultra-thin Al2O3 ceramic substrates can better play its advantages and have broad application prospects in industrial production.
[0003] Traditional metallization methods are mainly AMB, DBC, TFC and methods based on these process improvements. These methods have the following problems: AMB requires a very high vacuum degree (< 10 -2 Pa); DBC requires the preparation of a uniform and dense oxide film with a thickness within a certain range on the Cu surface in advance, which places high demands on the control of the preparation process; TFC requires the use of precious metal raw materials, which increases the process cost. In addition, most of the copper layers obtained by common metallization methods currently have problems such as low bonding strength, easy oxidation, uneven quality, and easy damage to ultra-thin ceramic substrates, which have great limitations in actual production applications.
[0004] In summary, it is imperative to find a method with low cost, simple process, high copper layer adhesion strength, uniform and dense copper layer quality and not easy to damage the ultra-thin ceramic substrate. Based on this, the present invention proposes a method of copper oxide sintering reduction metallization and pulse electroplating densification to solve the above problems. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide a low-cost metallization method for applying a densified copper layer on an ultra-thin ceramic substrate in response to the defects of the background technology. The method does not use precious metal raw materials, has a simple preparation process, low process cost, and the prepared metal layer is dense, has high bonding strength, and has intact substrate structural performance.
[0006] The present invention adopts the following technical solution to solve the above technical problems: a process for metallizing copper and densifying an ultra-thin Al2O3 ceramic substrate, comprising the following steps: Step 1: Use an ultrasonic cleaning machine to degrease and dry the ultra-thin ceramic substrate; Step 2: Using turpentine alcohol and dibutyl phthalate as solvents, ethyl cellulose M9 as a thickener, castor oil as a thixotropic agent, and PEG-400 as a surfactant, stir the above raw materials under heating conditions until they form a viscous and clear state as an organic carrier. Add CuO powder into the organic carrier to prepare CuO slurry; Step 3: Printing the copper oxide slurry on the surface of the ultra-thin Al2O3 ceramic substrate by coating or screen printing, and drying the ultra-thin Al2O3 ceramic substrate printed with the copper oxide slurry; Step 4: subjecting the dried substrate to a binder removal sintering process in an air atmosphere; cooling down after the sintering process, replacing the atmosphere in the atmosphere furnace with a reducing atmosphere for a reduction process, reducing CuO to metallic copper, and obtaining an ultra-thin Al2O3 ceramic substrate covered with metallic copper after the furnace temperature drops to room temperature; Step 5: Prepare the electroplating solution with copper sulfate pentahydrate, sodium chloride, sulfuric acid as the basic plating solution, PEG-6000 as the inhibitor, and JGB as the leveling agent; Step 6: Use an electroplating device to perform pulse electroplating densification, and place the anode copper plate and the cathode copper-clad ceramic substrate in the above electroplating solution at the same time, and perform electroplating under heating and stirring at 60°C; Step 7: After the electroplating is completed, take out the ceramic substrate, clean the surface plating solution with deionized water, and then soak and clean it with alcohol.
[0007] Preferably, in step 1, the thickness of the ultra-thin ceramic substrate is 100 μm to 200 μm, and the purity is one of 99%, 96%, 95%, and 90% by mass.
[0008] Preferably, in step 2, the CuO powder content is 80 wt.% to 85 wt.% of the slurry mass.
[0009] Preferably, in step 2, in the organic carrier, the amount of ethyl cellulose M9 added is 2wt.%~5wt.% of the organic carrier, the amount of castor oil added is 1wt.%~5wt.% of the organic carrier, the amount of PEG-400 added is 1wt.%~5wt.% of the organic carrier, the amount of dibutyl phthalate added is 1wt.%~4wt.% of the organic carrier, and the rest is turpentine alcohol.
[0010] Preferably, in step three, the CuO film prepared by screen printing or coating process has a thickness of 10 μm to 100 μm.
[0011] Preferably, in step three, the drying process temperature is 80° C. and the drying time is 0.5 h to 2 h.
[0012] Preferably, in step 4, the debinding process temperature is 350°C~600°C, and the holding time is 0.5h~2h; the sintering process temperature is 1070°C~1100°C, and the sintering time is 5min~2h; the reduction process temperature is 400°C~1000°C, and the reduction time is 2h~5h.
[0013] Preferably, in step 4, the reducing atmosphere is a nitrogen-hydrogen mixture (20% hydrogen).
[0014] Preferably, in step five, the content of copper sulfate pentahydrate is 150-250 g / L of the electroplating solution, the content of sodium chloride is 50-80 mg / L of the electroplating solution, the content of sulfuric acid is 30-100 g / L of the electroplating solution, the content of PEG-6000 is 50-500 mg / L of the electroplating solution, and the content of JGB is 5-10 mg / L of the electroplating solution.
[0015] Preferably, in step six, the average forward current density of pulse electroplating is 1ASD~5ASD, the duty cycle is 70%~90%, the frequency is 1kHz, the forward and reverse potential ratio is 1:2~1:5, and the electroplating time is 30min~5h.
[0016] Preferably, in step seven, the ceramic substrate after preliminary cleaning with deionized water is placed in alcohol and ultrasonically cleaned for 10 minutes to remove the surface plating solution to prevent contamination and corrosion of the plating solution.
[0017] The beneficial effects of the present invention are: (1) It fills the gap in the metallization process of ultra-thin ceramic substrates. The metallization process is simple, the obtained metal copper layer is not easy to oxidize, and has high bonding strength.
[0018] (2) The electroplating densification process makes up for the defect of high porosity of the copper layer obtained by the CuO sintering reduction copper coating method, improves the density of the metal layer, and optimizes the quality of the copper layer.
[0019] (3) The process temperature of the present invention is low, the process window is wide, the requirements for the accuracy of temperature, time and electroplating parameters are not high, the requirements for production equipment are low, and the process cost is low. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0021] Figure 1 A schematic diagram of the copper metallization of the ultra-thin Al2O3 ceramic substrate of the present invention; Figure 2 This is a scanning electron microscope image of the surface of the metallized copper-clad layer of the ultra-thin Al2O3 ceramic substrate of the present invention; Figure 3 A microscope schematic diagram of a cross section of the metallized copper-clad layer of the ultra-thin Al2O3 ceramic substrate of the present invention; DETAILED DESCRIPTION
[0022] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0023] The present invention discloses a copper-plating process for metallization of an ultra-thin Al2O3 ceramic substrate, which comprises at least the following steps: Step 1: Use an ultrasonic cleaning machine to degrease and dry the ultra-thin ceramic substrate; Step 2: Using turpentine alcohol and dibutyl phthalate as solvents, ethyl cellulose M9 as a thickener, castor oil as a thixotropic agent, and PEG-400 as a surfactant, stir the above raw materials under heating conditions until they form a viscous and clear state as an organic carrier. Add CuO powder into the organic carrier to prepare CuO slurry; Step 3: Printing the copper oxide slurry on the surface of the ultra-thin Al2O3 ceramic substrate by coating or screen printing, and drying the ultra-thin Al2O3 ceramic substrate printed with the copper oxide slurry; Step 4: subjecting the dried substrate to a binder removal sintering process in an air atmosphere; cooling down after the sintering process, replacing the atmosphere in the atmosphere furnace with a reducing atmosphere for a reduction process, reducing CuO to metallic copper, and obtaining an ultra-thin Al2O3 ceramic substrate covered with metallic copper after the furnace temperature drops to room temperature; Step 5: Prepare the electroplating solution with copper sulfate pentahydrate, sodium chloride, sulfuric acid as the basic plating solution, PEG-6000 as the inhibitor, and JGB as the leveling agent; Step 6: Use an electroplating device to perform pulse electroplating densification. The anode copper plate and the cathode copper-clad ceramic substrate are placed in the above-mentioned electroplating solution at the same time, and electroplating is performed under heating and stirring at 60°C.
[0024] Step 7: After the electroplating is completed, take out the ceramic substrate, clean the surface plating solution with deionized water, and then soak and clean it with alcohol for 10 minutes.
[0025] Example 1
[0026] Step 1: Prepare several 20×30 mm ultra-thin Al2O3 ceramic substrates, ultrasonically clean them in alcohol for 3 min and dry them; Step 2: Take 1.75g ethyl cellulose M9, 1.5g castor oil, 1.0g dibutyl phthalate, 1.5g PEG-400, and 33.25g turpentine, stir the above raw materials at 70°C with magnetic stirring until a viscous, clear, transparent light yellow solution is obtained as an organic carrier; mix 2g CuO powder with 0.5g organic carrier, and stir to prepare copper oxide slurry; Step 3: Print the copper oxide slurry on the surface of the ultra-thin Al2O3 ceramic substrate using a screen printing process, and dry the ultra-thin Al2O3 ceramic substrate printed with the copper oxide slurry at 80° C. until the surface slurry solidifies; Step 4: Place the dried substrate into a muffle furnace, heat it to 500°C at a rate of 10°C / min, and keep it warm for 40 minutes to completely remove the organic carrier in the copper oxide layer; Step 5: In an air atmosphere, the substrate is heated to 1080°C at a rate of 10°C / min, kept at that temperature for 30 minutes, and then cooled to room temperature in the furnace; Step 6: Place the above-mentioned sintered over-thick ultra-thin Al2O3 ceramic substrate in an atmosphere furnace, replace the atmosphere with a nitrogen-hydrogen mixed gas for a reduction process, heat up to 1000°C at a rate of 10°C / min, keep warm for 120 minutes, and then naturally cool to room temperature with the furnace; Step 7: Take 110g of copper sulfate pentahydrate and 25mg of sodium chloride and dissolve them in 450mL of deionized water. After dissolution, slowly add 25g of sulfuric acid to the solution along the glass rod in small amounts and multiple times, stirring while adding. Finally, use deionized water to wash off the residual sulfuric acid on the glass rod. Take 150mg of PEG-6000 and 5mg of JGB and add them to the above basic plating solution. Stir well after calibrating to 500mL. Step 8: Use an electroplating device for pulse electroplating densification. Connect the copper plate to the anode with a metal clip and the cathode to the copper-clad ceramic substrate. Place them in the above-mentioned electroplating solution at the same time. Set the electroplating parameters as follows: average forward current density of 3ASD, duty cycle of 70%, frequency of 1kHz, forward and reverse potential ratio of 1:2, electroplating time of 95min, and perform electroplating under heating and stirring at 60°C.
[0027] Step 9: After the electroplating is completed, take out the ceramic substrate, clean the surface plating solution with deionized water, soak it in alcohol, and ultrasonically clean it for 10 minutes.
[0028] Reference Figure 1 The ultra-thin Al2O3 ceramic substrate copper layer prepared in Example 1 has a copper layer thickness of about 50 μm.
[0029] Example 2
[0030] Step 1: Prepare several 20×30 mm ultra-thin Al2O3 ceramic substrates, ultrasonically clean them in alcohol for 3 min and dry them; Step 2: Take 1.75g ethyl cellulose M9, 1.5g castor oil, 1.0g dibutyl phthalate, 1.5g PEG-400, and 33.25g turpentine, stir the above raw materials at 70°C with magnetic stirring until a viscous, clear, transparent light yellow solution is obtained as an organic carrier; mix 2.1g CuO powder with 0.5g organic carrier, and stir to prepare a copper oxide slurry; Step 3: Print the copper oxide slurry on the surface of the ultra-thin Al2O3 ceramic substrate using a screen printing process, and dry the ultra-thin Al2O3 ceramic substrate printed with the copper oxide slurry at 80° C. until the surface slurry solidifies; Step 4: Place the dried substrate into a muffle furnace, heat it to 500°C at a rate of 10°C / min, and keep it warm for 40 minutes to completely remove the organic carrier in the copper oxide layer; Step 5: In an air atmosphere, the substrate is heated to 1075°C at a rate of 10°C / min, kept at this temperature for 30 minutes, and then cooled to room temperature in the furnace; Step 6: Place the above-mentioned sintered over-thick ultra-thin Al2O3 ceramic substrate in an atmosphere furnace, replace the atmosphere with a nitrogen-hydrogen mixed gas for a reduction process, heat up to 800°C at a rate of 10°C / min, keep warm for 120 minutes, and then naturally cool to room temperature with the furnace; Step 7: Take 110g of copper sulfate pentahydrate and 25mg of sodium chloride and dissolve them in 450mL of deionized water. After dissolution, slowly add 25g of sulfuric acid to the solution along the glass rod in small amounts and multiple times, stirring while adding. Finally, use deionized water to wash off the residual sulfuric acid on the glass rod. Take 150mg of PEG-6000 and 5mg of JGB and add them to the above basic plating solution. Stir well after calibrating to 500mL. Step 8: Use an electroplating device for pulse electroplating densification. Connect the copper plate to the anode with a metal clip and the cathode to the copper-clad ceramic substrate. Place them in the above-mentioned electroplating solution at the same time. Set the electroplating parameters as follows: average forward current density of 3ASD, duty cycle of 70%, frequency of 1kHz, forward and reverse potential ratio of 1:3, electroplating time of 125min, and perform electroplating under heating and stirring at 60°C.
[0031] Step 9: After the electroplating is completed, take out the ceramic substrate, clean the surface plating solution with deionized water, soak it in alcohol, and ultrasonically clean it for 10 minutes.
[0032] Example 3
[0033] Step 1: Prepare several 20×30 mm ultra-thin Al2O3 ceramic substrates, ultrasonically clean them in alcohol for 3 min and dry them; Step 2: Take 1.75g ethyl cellulose M9, 1.5g castor oil, 1.0g dibutyl phthalate, 1.5g PEG-400, and 33.25g turpentine, stir the above raw materials at 70°C with magnetic stirring until a viscous, clear, transparent light yellow solution is obtained as an organic carrier; mix 2.2g CuO powder with 0.5g organic carrier, and stir to prepare a copper oxide slurry; Step 3: Print the copper oxide slurry on the surface of the ultra-thin Al2O3 ceramic substrate using a screen printing process, and dry the ultra-thin Al2O3 ceramic substrate printed with the copper oxide slurry at 80° C. until the surface slurry solidifies; Step 4: Place the dried substrate into a muffle furnace, heat it to 500°C at a rate of 10°C / min, and keep it warm for 40 minutes to completely remove the organic carrier in the copper oxide layer; Step 5: In an air atmosphere, the substrate is heated to 1070°C at a rate of 10°C / min, kept at that temperature for 30 minutes, and then cooled to room temperature in the furnace; Step 6: Place the above-mentioned sintered over-thick ultra-thin Al2O3 ceramic substrate in an atmosphere furnace, replace the atmosphere with a nitrogen-hydrogen mixed gas for a reduction process, heat up to 600°C at a rate of 10°C / min, keep warm for 120min, and then naturally cool to room temperature with the furnace; Step 7: Take 110g of copper sulfate pentahydrate and 25mg of sodium chloride and dissolve them in 450mL of deionized water. After dissolution, slowly add 25g of sulfuric acid to the solution along the glass rod in small amounts and multiple times, stirring while adding. Finally, use deionized water to wash off the residual sulfuric acid on the glass rod. Take 150mg of PEG-6000 and 5mg of JGB and add them to the above basic plating solution. Stir well after calibrating to 500mL. Step 8: Use an electroplating device for pulse electroplating densification. Connect the copper plate to the anode with a metal clip and the cathode to the copper-clad ceramic substrate. Place them in the above-mentioned electroplating solution at the same time. Set the electroplating parameters as follows: average forward current density of 3ASD, duty cycle of 70%, frequency of 1kHz, forward and reverse potential ratio of 1:4, electroplating time of 180min, and perform electroplating under heating and stirring at 60°C.
[0034] Comparative Example 1 Step 1: Prepare several 20×30 mm ultra-thin Al2O3 ceramic substrates, ultrasonically clean them in alcohol for 3 min and dry them; Step 2: Take 1.75g ethyl cellulose M9, 1.5g castor oil, 1.0g dibutyl phthalate, 1.5g PEG-400, and 33.25g turpentine, stir the above raw materials at 70°C with magnetic stirring until a viscous, clear, transparent light yellow solution is obtained as an organic carrier; mix 2g CuO powder with 0.5g organic carrier, and stir to prepare copper oxide slurry; Step 3: Print the copper oxide slurry on the surface of the ultra-thin Al2O3 ceramic substrate using a screen printing process, and dry the ultra-thin Al2O3 ceramic substrate printed with the copper oxide slurry at 80° C. until the surface slurry solidifies; Step 4: Place the dried substrate into a muffle furnace, heat it to 500°C at a rate of 10°C / min, and keep it warm for 40 minutes to completely remove the organic carrier in the copper oxide layer; Step 5: In an air atmosphere, the substrate is heated to 1080°C at a rate of 10°C / min, kept at that temperature for 30 minutes, and then cooled to room temperature in the furnace; Step 6: Place the above-mentioned sintered over-thick ultra-thin Al2O3 ceramic substrate in an atmosphere furnace, replace the atmosphere with a nitrogen-hydrogen mixed gas for a reduction process, heat up to 1000°C at a rate of 10°C / min, keep warm for 120 minutes, and then naturally cool to room temperature with the furnace; Step 7: Take 110g of copper sulfate pentahydrate and 25mg of sodium chloride and dissolve them in 450mL of deionized water. After dissolution, slowly add 25g of sulfuric acid to the solution along the glass rod in small amounts and multiple times, stirring while adding. Finally, use deionized water to wash off the residual sulfuric acid on the glass rod. Take 150mg of PEG-6000 and 5mg of JGB and add them to the above basic plating solution. Stir well after calibrating to 500mL. Step 8: Use an electroplating device for pulse electroplating densification. Connect the copper plate to the anode with a metal clip and the cathode to the copper-clad ceramic substrate. Place them in the above-mentioned electroplating solution at the same time. Set the electroplating parameters as follows: average forward current density of 3ASD, duty cycle of 80%, frequency of 1kHz, forward and reverse potential ratio of 1:4, electroplating time of 125min, and perform electroplating under heating and stirring at 60°C.
[0035] Step 9: After the electroplating is completed, take out the ceramic substrate, clean the surface plating solution with deionized water, soak it in alcohol, and ultrasonically clean it for 10 minutes.
[0036] Comparative Example 2 Step 1: Prepare several 20×30 mm ultra-thin Al2O3 ceramic substrates, ultrasonically clean them in alcohol for 3 min and dry them; Step 2: Take 1.75g ethyl cellulose M9, 1.5g castor oil, 1.0g dibutyl phthalate, 1.5g PEG-400, and 33.25g turpentine, stir the above raw materials at 70°C with magnetic stirring until a viscous, clear, transparent light yellow solution is obtained as an organic carrier; mix 2g CuO powder with 0.5g organic carrier, and stir to prepare copper oxide slurry; Step 3: Print the copper oxide slurry on the surface of the ultra-thin Al2O3 ceramic substrate using a screen printing process, and dry the ultra-thin Al2O3 ceramic substrate printed with the copper oxide slurry at 80° C. until the surface slurry solidifies; Step 4: Place the dried substrate into a muffle furnace, heat it to 500°C at a rate of 10°C / min, and keep it warm for 40 minutes to completely remove the organic carrier in the copper oxide layer; Step 5: In an air atmosphere, the substrate is heated to 1080°C at a rate of 10°C / min, kept at that temperature for 30 minutes, and then cooled to room temperature in the furnace; Step 6: Place the above-mentioned sintered over-thick ultra-thin Al2O3 ceramic substrate in an atmosphere furnace, replace the atmosphere with a nitrogen-hydrogen mixed gas for a reduction process, heat up to 1000°C at a rate of 10°C / min, keep warm for 120 minutes, and then naturally cool to room temperature with the furnace; Step 7: Take 110g of copper sulfate pentahydrate and 25mg of sodium chloride and dissolve them in 450mL of deionized water. After dissolution, slowly add 25g of sulfuric acid to the solution along the glass rod in small amounts and multiple times, stirring while adding. Finally, use deionized water to wash off the residual sulfuric acid on the glass rod. Take 150mg of PEG-6000 and 5mg of JGB and add them to the above basic plating solution. Stir well after calibrating to 500mL. Step 8: Use an electroplating device for pulse electroplating densification. Connect the copper plate to the anode with a metal clip and the cathode to the copper-clad ceramic substrate. Place them in the above-mentioned electroplating solution at the same time. Set the electroplating parameters as follows: average forward current density of 3ASD, duty cycle of 90%, frequency of 1kHz, forward and reverse potential ratio of 1:4, electroplating time of 95min, and perform electroplating under heating and stirring at 60°C.
[0037] Step 9: After the electroplating is completed, take out the ceramic substrate, clean the surface plating solution with deionized water, soak it in alcohol, and ultrasonically clean it for 10 minutes.
[0038] The performance of the metallized alumina ceramic substrates prepared in the above Examples 1-3 and Comparative Examples 1-2 was tested, and the results are shown in Table 1:
[0039] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the technology may modify or change the above embodiments without violating the spirit and scope of the present invention. Therefore, all equivalent modifications or changes made by a person of ordinary skill in the art without departing from the spirit and technical ideas disclosed by the present invention are still covered by the claims of the present invention.
Claims
1. A process for copper metallization and densification of ultra-thin Al2O3 ceramic substrates, characterized in that: The method comprises: Substrate cleaning: Use an ultrasonic cleaner to physically remove oil from the surface of the ceramic substrate; Slurry preparation, preparing organic carrier and copper oxide slurry; Printing and coating, printing the copper oxide slurry on the surface of the ultra-thin Al2O3 ceramic substrate by coating or screen printing process and drying the ultra-thin Al2O3 ceramic substrate printed with the copper oxide slurry; Debinding, sintering, and reduction: the dried substrate is debinded and sintered in an air atmosphere; after sintering, the temperature is lowered, and the atmosphere in the atmosphere furnace is replaced with a reducing atmosphere for reduction, so that CuO is reduced to metallic copper, and after the furnace temperature drops to room temperature, an ultra-thin Al2O3 ceramic substrate covered with metallic copper is obtained; Pulse copper plating uses copper sulfate pentahydrate, sodium chloride, and sulfuric acid as the basic plating solution, PEG-6000 as the inhibitor, and JGB as the leveling agent to prepare the plating solution, and uses an electroplating device for pulse electroplating densification.
2. The process for metallization copper coating and densification of ultra-thin Al2O3 ceramic substrate according to claim 1, characterized in that: The thickness of the ultra-thin ceramic substrate is 100 μm to 200 μm, and the purity is one of 99%, 96%, 95%, and 90% by mass.
3. The process for metallization copper coating and densification of ultra-thin Al2O3 ceramic substrate according to claim 1, characterized in that: The CuO powder content is 80wt.%~85wt.% of the slurry mass.
4. The process for metallization copper coating and densification of ultra-thin Al2O3 ceramic substrate according to claim 1, characterized in that: The addition amount of ethyl cellulose M9 is 2wt.%~5wt.% of the organic carrier, the addition amount of castor oil is 1wt.%~5wt.% of the organic carrier, the addition amount of PEG-400 is 1wt.%~5wt.% of the organic carrier, the addition amount of dibutyl phthalate is 1wt.%~4wt.% of the organic carrier, and the rest is turpentine alcohol.
5. The process for metallization copper coating and densification of ultra-thin Al2O3 ceramic substrate according to claim 1, characterized in that: The CuO film prepared by screen printing or coating process has a thickness of 10μm~100μm.
6. The process for metallization copper coating and densification of ultra-thin Al2O3 ceramic substrate according to claim 1, characterized in that: The drying process temperature is 80°C and the drying time is 0.5h~2h.
7. The process for metallization copper coating and densification of ultra-thin Al2O3 ceramic substrate according to claim 1, characterized in that: The debinding process temperature is 350℃~600℃, and the holding time is 0.5h~2h; the sintering process temperature is 1070℃~1100℃, and the sintering time is 5min~2h; the reduction process temperature is 400℃~1000℃, and the reduction time is 2h~5h.
8. The process for metallization copper coating and densification of ultra-thin Al2O3 ceramic substrate according to claim 1, characterized in that: The reducing atmosphere is a nitrogen-hydrogen mixture (20% hydrogen).
9. The process for metallization copper coating and densification of ultra-thin Al2O3 ceramic substrate according to claim 1, characterized in that: The content of copper sulfate pentahydrate is 150-250 g / L of the electroplating solution, the content of sodium chloride is 50-80 mg / L of the electroplating solution, the content of sulfuric acid is 30-100 g / L of the electroplating solution, the content of PEG-6000 is 50-500 mg / L of the electroplating solution, and the content of JGB is 5-10 mg / L of the electroplating solution.
10. The process for metallization copper coating and densification of ultra-thin Al2O3 ceramic substrate according to claim 1, characterized in that: The average forward current density of pulse plating is 1ASD~5ASD, the duty cycle is 70%~90%, the frequency is 1kHz, the forward and reverse potential ratio is 1:2~1:5, and the plating time is 30min~5h.
Citation Information
Patent Citations
Manufacture method for copper-coated ceramic wafer on basis of electronic paste
CN102060573A
Fabrication method of printed circuit board
CN108207090A
Copper electroplating formula for pulse through hole filling and electroplating process thereof
CN114351195A
Metallic film resistor and its manufacture
JP1998092602A