Preparation method of high-functionality ultraviolet curing monomer and curing coating
Through the preparation method of high-functional ultraviolet cured monomer, a UV cured film with high crosslinking and wear resistance is generated by the reaction of isocyanate groups and acryloyloxy groups, which solves the lack of wear resistance of the UV cured film in the prior art. The problem of this paper achieves higher surface hardness and wear resistance, while simplifying the production process.
Patent Information
- Application Number
- CN202410977708.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-12
AI Technical Summary
Optimizing the formulation of UV cured films and improving the curing process in the prior art increases production difficulty and cost, and no effective solution has been proposed, resulting in insufficient wear resistance of UV cured films, especially in harsh environments.
A high-functional ultraviolet curing monomer preparation method is adopted. By reacting isocyanate groups and acryloyloxy groups, combining cyclohexanediol and catalysts, a high-functional monomer containing multiple acryloyloxy groups at both ends of the molecule is formed. Cured film with high crosslinking and wear resistance.
The surface hardness and wear resistance of the cured film are improved, the preparation route is simplified, the production cost is reduced, and the pressure reaction equipment is not required, which solves the problems of production difficulty and cost in the prior art.
Smart Images

Figure BDA0004955069080000051 
Figure BDA0004955069080000052
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer materials, and in particular to a method for preparing a high-functionality ultraviolet curing monomer and a curing coating. Background Art
[0002] Ultraviolet light-cured coating (also called UV light-cured coating) refers to the use of ultraviolet light energy to trigger the decomposition of photoinitiators in UV coatings to produce free radicals or cations, which in turn causes a cross-linking and curing reaction between UV resins and UV monomers in the coating, and achieves the curing of the coating by forming chemical bonds.
[0003] UV-cured films generally have good wear resistance. After curing, it can form a relatively hard and dense coating, which can resist friction and wear to a certain extent. However, its wear resistance may also be affected by some factors. For example, the thickness of the film. If the thickness is thin, the wear resistance may be relatively weak; the degree of curing is also critical. Incomplete curing may lead to reduced wear resistance. In addition, the use environment and the nature of the objects in contact will also affect the wear resistance. For example, in a harsh environment with a lot of sand and dust or sharp objects, the film may be more susceptible to wear.
[0004] In the prior art, when UV coatings are applied to high-performance applications, it is usually necessary to further improve the wear resistance of UV-cured films, such as by optimizing the formula, improving the curing process, and properly managing the use environment. However, when optimizing the formula, new anti-scratch agents and wear-resistant agents need to be added, which undoubtedly increases the complexity of the formula and production costs; and improving the curing process requires precise control and optimization of production equipment and operating techniques, such as precise control of light intensity and illumination time, which undoubtedly increases production costs and difficulty.
[0005] At present, no effective solution has been proposed for the problem that optimizing the formula and improving the curing process in the existing technology increase the difficulty and cost of production. Summary of the invention
[0006] In view of this, the embodiments of the present invention provide a method for preparing a high-functionality UV-curable monomer and a UV-curable coating, so as to at least solve the problem in the prior art that optimizing the formula and improving the curing process increase the production difficulty and cost.
[0007] The embodiment of the present invention provides the following technical solutions:
[0008] The embodiment of the present invention provides a method for preparing a high-functionality ultraviolet curing monomer, comprising:
[0009] Step 1, providing a first reaction product having an isocyanate group at one end and three acryloyloxy groups at the other end;
[0010] Step 2: After dissolving the first reaction product in a solvent, cyclohexanediol and a catalyst are added to the solvent respectively, the temperature is raised to a first reaction temperature, and after reacting for a first reaction time, a second reaction product having 6 acryloyloxy groups at both ends of the molecule is obtained, wherein, by weight, the first reaction product is 90 to 180 parts, the cyclohexanediol is 10 to 20 parts, the solvent is 60 to 100 parts, and the catalyst is 0.01 to 0.1 parts;
[0011] Step three: removing the solvent at a third reaction temperature to obtain the second reaction product, wherein the second reaction product has a high-functionality structure and a cyclic structure composed of an aliphatic ring.
[0012] Furthermore, the catalyst is at least one of dibutyltin dilaurate, stannous octoate, triphenylphosphine and triethylamine; and the solvent is ethyl acetate.
[0013] Furthermore, the first reaction product and the cyclohexanediol satisfy a molar ratio of isocyanate group to primary hydroxyl group of 1:(2-3).
[0014] Furthermore, the first reaction temperature is 70-90°C.
[0015] Furthermore, the first reaction time is 2 hours.
[0016] Furthermore, before step 1, the method further includes:
[0017] The isophorone diisocyanate is heated to a second reaction temperature under nitrogen protection, and pentaerythritol triacrylate is added dropwise to obtain a first reaction product after a second reaction time. The first reaction product has an isocyanate structure at one end and three acryloyloxy groups at the other end.
[0018] Furthermore, the molar ratio of the pentaerythritol triacrylate to the isophorone diisocyanate is 1:(1-2).
[0019] Furthermore, the second reaction temperature is 30-50°C.
[0020] An embodiment of the present invention also provides a UV-curable coating, comprising the second reaction product prepared by any of the above methods for preparing high-functionality UV-curable monomers, wherein the UV-curable coating also comprises hydroxyethyl methacrylate, a wetting agent, a leveling agent, a defoaming agent, and a photoinitiator.
[0021] Furthermore, in parts by mass, the hydroxyethyl methacrylate is 30 parts, the second reaction product is 10 to 45 parts, the wetting agent is 1 part, the leveling agent is 0.05 parts, the defoaming agent is 0.2 parts, and the photoinitiator is 6 parts.
[0022] Compared with the prior art, the at least one technical solution adopted in the embodiment of the present invention can achieve the following beneficial effects:
[0023] The invention discloses a method for preparing a high-functionality ultraviolet-curing monomer, comprising providing a first reaction product having an isocyanate group at one end and three acryloyloxy groups at the other end; dissolving the first reaction product in a solvent, respectively adding cyclohexanediol and a catalyst into the solvent, raising the temperature to a first reaction temperature, and reacting for a first reaction time to obtain a second reaction product having six acryloyloxy groups at both ends of the molecule, wherein, by weight, the first reaction product is 90 to 180 parts, the cyclohexanediol is 10 to 20 parts, the solvent is 60 to 100 parts, and the catalyst is 0.01 to 0.1 parts; removing the solvent at a third reaction temperature to obtain the second reaction product (ultraviolet-curing monomer), wherein the obtained second reaction product contains a high-functionality multi-structure and a transposed structure composed of an aliphatic ring, so that the molecular network structure of the formed cured film has better crosslinking degree, wear resistance and heat resistance, and the surface hardness and wear resistance of the formed cured film are higher. The invention has a short preparation route, a low reaction temperature, and does not require a pressure reaction device, thereby solving the problem that the optimization of the formula and the improvement of the curing process in the prior art increase the production difficulty and cost. DETAILED DESCRIPTION
[0024] The following describes the implementation methods of the present application through specific examples, and those skilled in the art can easily understand other advantages and effects of the present application from the contents disclosed in this specification. Obviously, the described embodiments are only a part of the embodiments of the present application, rather than all the embodiments. The present application can also be implemented or applied through other different specific implementation methods, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present application. It should be noted that, in the absence of conflict, the following embodiments and the features in the embodiments can be combined with each other. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in the field without making creative work belong to the scope of protection of the present application.
[0025] It should be noted that various aspects of the embodiments within the scope of the appended claims are described below. It should be apparent that the aspects described herein can be embodied in a wide variety of forms, and any specific structure and / or function described herein is merely illustrative. Based on the present application, it should be understood by those skilled in the art that an aspect described herein can be implemented independently of any other aspect, and two or more of these aspects can be combined in various ways. For example, any number and aspect described herein can be used to implement the device and / or practice the method. In addition, other structures and / or functionalities other than one or more of the aspects described herein can be used to implement this device and / or practice this method.
[0026] Additionally, in the following description, specific details are provided to facilitate a thorough understanding of the examples. However, it will be understood by those skilled in the art that the examples can be practiced without these specific details.
[0027] In the field of high-performance use of UV coatings, it is often necessary to further improve the wear resistance of UV-cured films according to actual use needs. Usually, improvements can be made from aspects such as optimizing the formula, improving the curing process, and properly managing the use environment to improve the wear resistance of UV-cured films.
[0028] When optimizing the formula, wear-resistant additives can be added, such as anti-scratch agents, wear-resistant agents, etc. These additives can enhance the wear resistance of the coating. Since fumed silica is an inorganic non-metallic material with excellent physiological inertness, it will be added to the UV light-curing coating. When the addition amount reaches more than 3%, the hardness and strength of the UV coating can be significantly improved, thereby improving the wear resistance of the coating.
[0029] When improving the curing process, it is usually necessary to optimize the process parameters of UV light curing, such as light intensity, illumination time, etc., which may also affect the wear resistance.
[0030] Since it is more valuable to improve the wear resistance of UV curing film in the network structure of UV curing film itself, it is necessary to develop a high-functionality UV monomer that can cure quickly, has good wear resistance and strong scratch resistance, so that it can be connected to the cured network structure after curing to play a wear-resistant role.
[0031] Based on this, the embodiment of this specification proposes a processing scheme: a method for preparing a high-functionality UV-curable monomer of the present invention, wherein the first reaction product reacts with cyclohexanediol in a solvent through a catalyst (a mixture of one or more of dibutyltin dilaurate, stannous octoate, triphenylphosphine, and triethylamine), and reacts at a first preset temperature for a first reaction time, thereby obtaining a second reaction product, that is, a second reaction product having a high-functionality multi-structure and a remodeling structure composed of aliphatic rings.
[0032] The technical solutions provided by each embodiment of the present application are described in detail below.
[0033] Example 1
[0034] This embodiment provides a method for preparing a high-functionality ultraviolet-curable monomer, which is suitable for UV-LED light source irradiation curing, and the formed cured film has high surface hardness and wear resistance. The method for preparing a high-functionality ultraviolet-curable monomer comprises:
[0035] Step 1: providing a first reaction product having an isocyanate group at one end and three acryloyloxy groups at the other end.
[0036] Furthermore, the method for obtaining the first reaction product comprises the following steps:
[0037] The isophorone diisocyanate is heated to a second reaction temperature under nitrogen protection, and pentaerythritol triacrylate is added dropwise. After a second reaction time, a first reaction product is obtained. The first reaction product has an isocyanate structure at one end and three acryloyloxy groups at the other end.
[0038] Specifically, the equation for obtaining the first reaction product is as follows:
[0039]
[0040] In some of the embodiments, the first reaction product can also be obtained from other materials, such as cyanurate and acrylate containing multiple hydroxyl groups, trifunctional isocyanate and acrylate monomers, etc.
[0041] Furthermore, the molar ratio of pentaerythritol triacrylate to isophorone diisocyanate is 1:(1-2).
[0042] Preferably, the molar ratio of pentaerythritol triacrylate to isophorone diisocyanate is 1:(1-1.5).
[0043] More preferably, the molar ratio of pentaerythritol triacrylate to isophorone diisocyanate is 1:(1-1.3).
[0044] Most preferably, the molar ratio of pentaerythritol triacrylate to isophorone diisocyanate is 1:(1-1.2).
[0045] Furthermore, the second reaction temperature is 30-50°C.
[0046] Preferably, the second reaction temperature is 30-40°C.
[0047] Step 2: After dissolving the first reaction product in a solvent, cyclohexanediol and a catalyst are added to the solvent respectively, the temperature is raised to a first reaction temperature, and after reacting for a first reaction time, a second reaction product containing 6 acryloyloxy groups at both ends of the molecule is obtained, wherein, by mass, the first reaction product is 90 to 180 parts, the cyclohexanediol is 10 to 20 parts, the solvent is 60 to 100 parts, and the catalyst is 0.01 to 0.1 parts.
[0048] Wherein, the chemical formula of the second reaction product is as follows:
[0049]
[0050] Furthermore, the catalyst is at least one of dibutyltin dilaurate, stannous octoate, triphenylphosphine and triethylamine; and the solvent is ethyl acetate.
[0051] Furthermore, the first reaction product and cyclohexanediol satisfy a molar ratio of isocyanate group to primary hydroxyl group of 1:(2-3).
[0052] Furthermore, the first reaction product and cyclohexanediol satisfy a molar ratio of isocyanate group to primary hydroxyl group of 1:(2-2.5).
[0053] Preferably, the first reaction product and cyclohexanediol satisfy a molar ratio of isocyanate group to primary hydroxyl group of 1:(2-2.2).
[0054] Furthermore, the first reaction temperature is 70-90°C.
[0055] Preferably, the first reaction temperature is 75-85°C.
[0056] Furthermore, the first reaction time is 1 to 2 hours.
[0057] Step 3: removing the solvent at a third reaction temperature to obtain a second reaction product, wherein the second reaction product has a high-functionality structure and a cyclic structure composed of an aliphatic ring.
[0058] The second reaction product is a high-functionality ultraviolet monomer.
[0059] In this example, each component is added into a container in sequence, stirred at 70-90° C. for 1-2 hours, and then vacuum-dried to remove the solvent, thereby obtaining a high-functionality UV monomer (second reaction product).
[0060] The following are several specific implementation methods of this embodiment:
[0061] Implementation Method 1
[0062] Step 1. Add 111 g of isophorone diisocyanate (IPDI) into a 500 mL four-necked flask equipped with a thermometer and a condenser, and heat the isophorone diisocyanate to 30° C. under nitrogen protection, and start the stirrer; slowly dropwise add 150 g of pentaerythritol triacrylate from which water has been removed, and react for 1 hour; obtain a first reaction product having an isocyanate structure at one end of the molecule and three acryloyloxy groups at the other end;
[0063] Step 2. Add 90 g of the first reaction product containing an isocyanate structure at one end and three acryloyloxy groups at the other end prepared in step 1 into a 500 mL four-necked flask with a thermometer and a condenser, add 60 g of ethyl acetate to the flask, and simultaneously add 10 g of cyclohexanediol and 0.01 g of dibutyltin dilaurate (catalyst) to the flask, then slowly increase the temperature to 70 ° C and continue the reaction for 2 hours. After the reaction is completed, remove the ethyl acetate at 40 ° C under a vacuum degree of 0.093 MPa, and finally obtain a high-functionality UV monomer product (second reaction product).
[0064] Implementation Method 2
[0065] Step 1. Add 111 g of isophorone diisocyanate (IPDI) into a 500 mL four-necked flask equipped with a thermometer and a condenser, heat to 50° C. under nitrogen protection, and start the stirrer; slowly dropwise add 150 g of pentaerythritol triacrylate from which water has been removed, and react for 1 hour; obtain a first reaction product having an isocyanate structure at one end of the molecule and three acryloyloxy groups at the other end;
[0066] Step 2. Add 180 g of the first reaction product containing an isocyanate structure at one end and three acryloyloxy groups at the other end prepared in step 1 into a 500 mL four-necked flask with a thermometer and a condenser, add 100 g of ethyl acetate to the flask, and simultaneously add 20 g of cyclohexanediol and 0.1 g of dibutyltin dilaurate (catalyst) to the flask, then slowly increase the temperature to 90°C and continue the reaction for 2 hours. After the reaction is completed, remove the ethyl acetate at 40°C under a vacuum degree of 0.093 MPa, and finally obtain a high-functionality UV monomer product (second reaction product).
[0067] Implementation 3
[0068] Step 1: Add 111 g of isophorone diisocyanate (IPDI) into a 500 mL four-necked flask equipped with a thermometer and a condenser, heat to 35° C. under nitrogen protection, and start the stirrer; slowly dropwise add 150 g of pentaerythritol triacrylate from which water has been removed, and react for 1 hour; obtain a first reaction product having an isocyanate structure at one end of the molecule and three acryloyloxy groups at the other end;
[0069] Step 2: Add 150g of the first reaction product prepared in step 1, which has an isocyanate structure at one end of the molecule and three acryloyloxy groups at the other end, into a 500mL four-necked flask with a thermometer and a condenser, add 80g of ethyl acetate into the flask, and simultaneously add 15g of cyclohexanediol and 0.05g of dibutyltin dilaurate (catalyst) into the flask, then slowly increase the temperature to 75°C and continue the reaction for 2h. After the reaction is completed, remove the ethyl acetate at 40°C under a vacuum degree of 0.093MPa, and finally obtain a high-functionality UV monomer product (second reaction product).
[0070] According to the above embodiment, after obtaining the first reaction product, the first reaction product is dissolved in ethyl acetate and then reacted with cyclohexanediol under the action of a catalyst to obtain a second reaction product, that is, an ultraviolet monomer product; and the above embodiment also proves that step two can normally obtain an ultraviolet monomer product at 70 to 90°C / catalyst at 0.01 to 0.1g.
[0071] Compared with the prior art, the molecular structure of the high-functionality UV monomer of the present invention contains a high-functionality multi-structure and a conversion structure composed of aliphatic rings. Therefore, the molecular network structure of the cured film formed by the UV monomer of this embodiment has higher cross-linking, wear resistance and heat resistance, which can make the surface hardness and wear resistance of the cured film higher.
[0072] The method for preparing ultraviolet monomers of the present invention has the advantages of short preparation line, low reaction temperature, no need for pressure reaction equipment, simple preparation process, convenient operation, mild reaction conditions, and is suitable for industrial production.
[0073] Example 2
[0074] This embodiment provides a UV-curable coating, including a second reaction product prepared by the method for preparing a high-functionality UV-curable monomer as described in Example 1, and the UV-curable coating also includes hydroxyethyl methacrylate, a wetting agent, a leveling agent, a defoaming agent, and a photoinitiator.
[0075] Furthermore, by mass, 30 parts of hydroxyethyl methacrylate, 10 to 45 parts of the second reaction product, 1 part of a wetting agent, 0.05 parts of a leveling agent, 0.2 parts of a defoaming agent, and 6 parts of a photoinitiator are used.
[0076] The invention provides a highly wear-resistant UV coating by dispersing the second reaction product, a wetting agent, a leveling agent, a defoaming agent, a photoinitiator, and UV light-curing resins B210-D, B-6019, and B-2116 for 30 minutes and mixing them evenly, and then a highly wear-resistant UV coating is obtained, and a highly wear-resistant UV film is obtained after UV curing. The high-functionality UV monomer prepared by the invention has the characteristics of being able to effectively improve the wear-resistant effect of the UV-curing film and improving the scratch resistance level, and the prepared UV-curing film has good wear resistance and scratch resistance.
[0077] The following are various specific implementations of this embodiment:
[0078] Implementation Method 1
[0079] In a GFJ-0.4 high-speed disperser, 30 parts of hydroxyethyl methacrylate, 10 parts of the prepared high-functionality UV monomer, 1 part of BYK333 wetting agent, 0.05 parts of BYK-345 leveling agent, 0.2 parts of BYK-024 defoaming agent, and 6 parts of TPO photoinitiator were added. After dispersing at a speed of 600 r / min for 15 minutes, the speed was reduced to 300 r / min, and 30 parts of B210-D, 30 parts of B-6019, and 20 parts of B-2116 were added. The dispersion was continued for 30 minutes and mixed evenly to obtain a high wear-resistant UV coating. After curing, a high wear-resistant UV film was obtained.
[0080] The prepared nail polish sealant is evenly applied on the PS substrate using a wire rod applicator, and the coating thickness is controlled to be 20μm. After curing with a phototherapy lamp, 0000# steel wool is used as the wear test material. The velvet is tied to the wiping head of an automatic abrasion tester with a load of one kilogram. After wiping the paint film back and forth 20 times, the scratches on the film surface are observed through a mirror microscope.
[0081] According to GB / T6739-2006 "Determination of film hardness by pencil method for paints and varnishes", the hardness of the UV light-cured film obtained above was tested using a QHQ coating pencil scratch hardness tester. The test results are listed in Table 1 below.
[0082] Implementation Method 2
[0083] In a GFJ-0.4 high-speed disperser, 30 parts of hydroxyethyl methacrylate, 20 parts of the prepared high-functionality UV monomer, 1 part of BYK333 wetting agent, 0.05 parts of BYK-345 leveling agent, 0.2 parts of BYK-024 defoaming agent, and 6 parts of TPO photoinitiator were added. After dispersing at a speed of 600 r / min for 15 minutes, the speed was reduced to 300 r / min, and 30 parts of B210-D, 30 parts of B-6019, and 20 parts of B-2116 were added. The dispersion was continued for 30 minutes and mixed evenly to obtain a high wear-resistant UV coating. After curing, a high wear-resistant UV film was obtained.
[0084] The prepared nail polish sealant is evenly applied on the PS substrate using a wire rod applicator, and the coating thickness is controlled to be 20μm. After curing with a phototherapy lamp, 0000# steel wool is used as the wear test material. The velvet is tied to the wiping head of an automatic abrasion tester with a load of one kilogram. After wiping the paint film back and forth 20 times, the scratches on the film surface are observed through a mirror microscope.
[0085] According to GB / T6739-2006 "Determination of film hardness by pencil method for paints and varnishes", the hardness of the UV light-cured film obtained above was tested using a QHQ coating pencil scratch hardness tester. The test results are listed in Table 1 below.
[0086] Implementation 3
[0087] In a GFJ-0.4 high-speed disperser, 30 parts of hydroxyethyl methacrylate, 30 parts of the prepared high-functionality UV monomer, 1 part of BYK333 wetting agent, 0.05 parts of BYK-345 leveling agent, 0.2 parts of BYK-024 defoaming agent, and 6 parts of TPO photoinitiator were added. After dispersing at a speed of 600 r / min for 15 minutes, the speed was reduced to 300 r / min, and 30 parts of B210-D, 30 parts of B-6019, and 20 parts of B-2116 were added. The dispersion was continued for 30 minutes and mixed evenly to obtain a high wear-resistant UV coating. After curing, a high wear-resistant UV film was obtained.
[0088] The prepared nail polish sealant is evenly applied on the PS substrate using a wire rod applicator, and the coating thickness is controlled to be 20μm. After curing with a phototherapy lamp, 0000# steel wool is used as the wear test material. The velvet is tied to the wiping head of an automatic abrasion tester with a load of one kilogram. After wiping the paint film back and forth 20 times, the scratches on the film surface are observed through a mirror microscope.
[0089] According to GB / T6739-2006 "Determination of film hardness by pencil method for paints and varnishes", the hardness of the UV light-cured film obtained above was tested using a QHQ coating pencil scratch hardness tester. The test results are listed in Table 1.
[0090] Implementation 4
[0091] In a GFJ-0.4 high-speed disperser, 30 parts of hydroxyethyl methacrylate, 35 parts of the prepared high-functionality UV monomer, 1 part of BYK333 wetting agent, 0.05 parts of BYK-345 leveling agent, 0.2 parts of BYK-024 defoaming agent, and 6 parts of TPO photoinitiator were added. After dispersing at a speed of 600 r / min for 15 minutes, the speed was reduced to 300 r / min, and 30 parts of B210-D, 30 parts of B-6019, and 20 parts of B-2116 were added. The dispersion was continued for 30 minutes and mixed evenly to obtain a high wear-resistant UV coating. After curing, a high wear-resistant UV film was obtained.
[0092] The prepared nail polish sealant is evenly applied on the PS substrate using a wire rod applicator, and the coating thickness is controlled to be 20μm. After curing with a phototherapy lamp, 0000# steel wool is used as the wear test material. The velvet is tied to the wiping head of an automatic abrasion tester with a load of one kilogram. After wiping the paint film back and forth 20 times, the scratches on the film surface are observed through a mirror microscope.
[0093] According to GB / T6739-2006 "Determination of film hardness by pencil method for paints and varnishes", the hardness of the UV light-cured film obtained above was tested using a QHQ coating pencil scratch hardness tester. The test results are listed in Table 1.
[0094] Implementation method 5
[0095] In a GFJ-0.4 high-speed disperser, 30 parts of hydroxyethyl methacrylate, 40 parts of the prepared high-functionality UV monomer, 1 part of BYK333 wetting agent, 0.05 parts of BYK-345 leveling agent, 0.2 parts of BYK-024 defoaming agent, and 6 parts of TPO photoinitiator were added. After dispersing at a speed of 600 r / min for 15 minutes, the speed was reduced to 300 r / min, and 30 parts of B210-D, 30 parts of B-6019, and 20 parts of B-2116 were added. The dispersion was continued for 30 minutes and mixed evenly to obtain a high wear-resistant UV coating. After curing, a high wear-resistant UV film was obtained.
[0096] The prepared nail polish sealant is evenly applied on the PS substrate using a wire rod applicator, and the coating thickness is controlled to be 20μm. After curing with a phototherapy lamp, 0000# steel wool is used as the wear test material. The velvet is tied to the wiping head of an automatic abrasion tester with a load of one kilogram. After wiping the paint film back and forth 20 times, the scratches on the film surface are observed through a mirror microscope.
[0097] According to GB / T6739-2006 "Determination of film hardness by pencil method for paints and varnishes", the hardness of the UV light-cured film obtained above was tested using a QHQ coating pencil scratch hardness tester. The test results are listed in Table 1.
[0098] Implementation 6
[0099] In a GFJ-0.4 high-speed disperser, 30 parts of hydroxyethyl methacrylate, 45 parts of the prepared high-functionality UV monomer, 1 part of BYK333 wetting agent, 0.05 parts of BYK-345 leveling agent, 0.2 parts of BYK-024 defoaming agent, and 6 parts of TPO photoinitiator were added. After dispersing at a speed of 600 r / min for 15 minutes, the speed was reduced to 300 r / min, and 30 parts of B210-D, 30 parts of B-6019, and 20 parts of B-2116 were added. The dispersion was continued for 30 minutes and mixed evenly to obtain a high wear-resistant UV coating. After curing, a high wear-resistant UV film was obtained.
[0100] The prepared nail polish sealant is evenly applied on the PS substrate using a wire rod applicator, and the coating thickness is controlled to be 20μm. After curing with a phototherapy lamp, 0000# steel wool is used as the wear test material. The velvet is tied to the wiping head of an automatic abrasion tester with a load of one kilogram. After wiping the paint film back and forth 20 times, the scratches on the film surface are observed through a mirror microscope.
[0101] According to GB / T6739-2006 "Determination of film hardness by pencil method for paints and varnishes", the hardness of the UV light-cured film obtained above was tested using a QHQ coating pencil scratch hardness tester. The test results are listed in Table 1.
[0102] The following is a comparative implementation without adding the second reaction product of the present invention;
[0103] Comparative Example 1
[0104] Add 30 parts of hydroxyethyl methacrylate, 1 part of BYK333 wetting agent, 0.05 parts of BYK-345 leveling agent, 0.2 parts of BYK-024 defoaming agent, and 6 parts of TPO photoinitiator to a GFJ-0.4 high-speed disperser, disperse at 600 r / min for 15 minutes, then reduce the speed to 300 r / min, continue to add 30 parts of B210-D, 30 parts of B-6019, and 20 parts of B-2116, continue to disperse for 30 minutes, mix evenly, and obtain a high wear-resistant UV coating, which is cured to obtain a high wear-resistant UV film.
[0105] The prepared nail polish sealant is evenly applied on the PS substrate using a wire rod applicator, and the coating thickness is controlled to be 20μm. After curing with a phototherapy lamp, 0000# steel wool is used as the wear test material. The velvet is tied to the wiping head of an automatic abrasion tester with a load of one kilogram. After wiping the paint film back and forth 20 times, the scratches on the film surface are observed through a mirror microscope.
[0106] According to GB / T6739-2006 "Determination of film hardness by pencil method for paints and varnishes", the hardness of the UV light-cured film obtained above was tested using a QHQ coating pencil scratch hardness tester. The test results are listed in Table 1.
[0107] Comparative Example 2
[0108] In a GFJ-0.4 high-speed disperser, 40 parts of hydroxyethyl methacrylate, 1 part of BYK333 wetting agent, 0.05 parts of BYK-345 leveling agent, 0.2 parts of BYK-024 defoaming agent, and 6 parts of TPO photoinitiator were added. After dispersing at 600 r / min for 15 minutes, the speed was reduced to 300 r / min, and 30 parts of B210-D, 30 parts of B-6019, and 20 parts of B-2116 were added. The dispersion was continued for 30 minutes and mixed evenly to obtain a high wear-resistant UV coating. After curing, a high wear-resistant UV film was obtained.
[0109] The prepared nail polish sealant is evenly applied on the PS substrate using a wire rod applicator, and the coating thickness is controlled to be 20μm. After curing with a phototherapy lamp, 0000# steel wool is used as the wear test material. The velvet is tied to the wiping head of an automatic abrasion tester with a load of one kilogram. After wiping the paint film back and forth 20 times, the scratches on the film surface are observed through a mirror microscope.
[0110] According to GB / T6739-2006 "Determination of film hardness by pencil method for paints and varnishes", the hardness of the UV light-cured film obtained above was tested using a QHQ coating pencil scratch hardness tester. The test results are listed in Table 1.
[0111] sample Pencil hardness Number of scratches Implementation Method 1 H none Implementation Method 2 2H none Implementation 3 3H none Implementation 4 4H none Implementation method 5 4H none Implementation 6 4H none Comparative Example 1 HB 11 Comparative Example 2 HB 10
[0112] Table 1 Test results
[0113] According to the above comparative experiments and comparison of the embodiments of the coating, it can be seen that the UV-curable coating of the present invention has good abrasion resistance and scratch resistance compared with the prior art.
[0114] In this specification, the same or similar parts between the various embodiments can be referred to each other, and each embodiment focuses on the differences from other embodiments. In particular, for the product embodiment described later, since it corresponds to the method, the description is relatively simple, and the relevant parts can be referred to the partial description of the system embodiment.
[0115] The above is only a specific implementation of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application shall be based on the protection scope of the claims.
Claims
1. A method for preparing a high-functionality UV-curable monomer, characterized in that: include: Step 1, providing a first reaction product having an isocyanate group at one end and three acryloyloxy groups at the other end; Step 2: After dissolving the first reaction product in a solvent, cyclohexanediol and a catalyst are added to the solvent respectively, the temperature is raised to a first reaction temperature, and after reacting for a first reaction time, a second reaction product having 6 acryloyloxy groups at both ends of the molecule is obtained, wherein, by weight, the first reaction product is 90 to 180 parts, the cyclohexanediol is 10 to 20 parts, the solvent is 60 to 100 parts, and the catalyst is 0.01 to 0.1 parts; Step three: removing the solvent at a third reaction temperature to obtain the second reaction product, wherein the second reaction product has a high-functionality structure and a cyclic structure composed of an aliphatic ring.
2. The method for preparing a high-functionality UV-curable monomer according to claim 1, characterized in that: The catalyst is at least one of dibutyltin dilaurate, stannous octoate, triphenylphosphine and triethylamine; and the solvent is ethyl acetate.
3. The method for preparing a high-functionality UV-curable monomer according to claim 2, characterized in that: The molar ratio of isocyanate group to primary hydroxyl group between the first reaction product and the cyclohexanediol is 1:(2-3).
4. The method for preparing a high-functionality UV-curable monomer according to claim 3, characterized in that: The first reaction temperature is 70-90°C.
5. The method for preparing a high-functionality UV-curable monomer according to claim 4, characterized in that: The first reaction time is 2h.
6. The method for preparing a high-functionality ultraviolet curing monomer according to any one of claims 1 to 5, characterized in that: Before step 1, it also includes: The isophorone diisocyanate is heated to a second reaction temperature under nitrogen protection, and pentaerythritol triacrylate is added dropwise to obtain a first reaction product after a second reaction time. The first reaction product has an isocyanate structure at one end and three acryloyloxy groups at the other end.
7. The method for preparing a high-functionality UV-curable monomer according to claim 6, characterized in that: The molar ratio of the pentaerythritol triacrylate to the isophorone diisocyanate is 1:(1-2).
8. The method for preparing a high-functionality UV-curable monomer according to claim 7, characterized in that: The second reaction temperature is 30-50°C.
9. A UV curing coating, characterized in that: The second reaction product is prepared by the method for preparing a high-functionality UV-curable monomer as described in any one of claims 1 to 8, and the UV-curable coating further comprises hydroxyethyl methacrylate, a wetting agent, a leveling agent, a defoaming agent, and a photoinitiator.
10. The UV curing coating according to claim 9, characterized in that: In parts by mass, the hydroxyethyl methacrylate is 30 parts, the second reaction product is 10 to 45 parts, the wetting agent is 1 part, the leveling agent is 0.05 parts, the defoaming agent is 0.2 parts, and the photoinitiator is 6 parts.
Citation Information
Patent Citations
Photosensitive resin composition, photosensitive film, rib pattern formation method, hollow structure and formation method for same, and electronic component
CN102906641A
UV-curable high-functionality resin and preparation method thereof
CN104327247A
Light-cured water-based acrylic acid dispersion as well as preparation method and application thereof
CN112029067A
Hardened polyurethane acrylate adhesive and preparation method thereof
CN113817437A
Solvent-resistant waterborne polyurethane and preparation method thereof
CN114805743A