Preparation method of nickel complex catalyst and application of nickel complex catalyst in preparation of pentenenitrile by hydrocyanation of butadiene

By preparing a nickel-oxoanthracene type bidentate phosphine ligand complex catalyst, the problems of HCN toxicity and high temperature and pressure in the existing butadiene hydrocyanation process were solved, and high-yield and safe pentenenitrile production was achieved.

CN118930588AInactive Publication Date: 2024-11-12ZHENGZHOU UNIV +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202310534474.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-12
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing butadiene hydrocyanation process uses highly toxic HCN, which is difficult to transport. The application conditions of phosphite-type ligand catalysts are harsh, with high reaction temperatures and additional pressure required, resulting in high production costs and poor safety.

Method used

A nickel-bident phosphine ligand complex catalyst was prepared by mixing anoxanthracene-type bidentate phosphine ligands with nickel metal salts under anhydrous and oxygen-free conditions to form a nickel-bident phosphine ligand complex catalyst. The reaction conditions were mild (≤80℃, ~0.1MPa), and an auxiliary agent was added to regulate the reaction process.

Benefits of technology

The method achieves efficient preparation of pentenonitrile under mild conditions, with a total yield of ≥90% for 3/4-pentenonitrile and 2-methyl-3-butenonitrile, improving safety and production efficiency while reducing energy consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004225603890000022
    Figure BDA0004225603890000022
  • Figure BDA0004225603890000023
    Figure BDA0004225603890000023
  • Figure BDA0004225603890000041
    Figure BDA0004225603890000041
Patent Text Reader

Abstract

The invention belongs to the fields of adiponitrile preparation technology and olefin addition, relates to a preparation method of a nickel complex catalyst and application of the nickel complex catalyst in preparation of pentenenitrile by hydrocyanation of butadiene, and aims to solve the problems that in the prior art, in the butadiene hydrocyanation process, a raw material HCN is highly toxic and difficult to transport, and the cost is low. The application condition of a phosphite type ligand catalyst is harsh, the preparation process of an effective complex catalyst is not clear, the reaction temperature is relatively high, and additional pressurization is needed. The invention provides a nickel complex catalyst for preparing pentenenitrile by hydrocyanation of butadiene, the nickel complex catalyst is a nickel-bidentate phosphine ligand-assistant complex catalyst, and under anhydrous and anaerobic conditions, alcohol, butadiene and trimethylsilyl cyanide are sequentially added into the prepared nickel complex catalyst solution for sealed reaction, and the nickel complex catalyst is obtained. After the reaction is finished, the temperature is rapidly cooled to the room temperature, pentenenitrile is obtained, the pentenenitrile is 3 / 4 pentenenitrile and 2-methyl-3-butenenitrile, and the highest total yield can reach 95.69%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of adiponitrile preparation technology and olefin addition, and relates to a method for preparing a nickel complex catalyst and application of the nickel complex catalyst in preparing pentenenitrile by hydrocyanation of butadiene. Background Art

[0002] Adiponitrile is an important intermediate for the synthesis of nylon 66. The process is to hydrogenate adiponitrile to generate hexamethylenediamine, which is then neutralized with adipic acid to generate nylon 66. At present, the core production technology of adiponitrile is in the hands of a few large foreign companies. With the rapid development of my country's economy, the demand for various nylon 66 products is increasing. At present, my country's adiponitrile production capacity is insufficient to meet the needs of the domestic market and is heavily dependent on imports. Therefore, it has become an important issue to promote the development and application of adiponitrile localization technology, break the monopoly of foreign technology, and promote the rapid development of my country's nylon 66 industry.

[0003] At present, the main process routes for producing adiponitrile worldwide are acrylonitrile electrolytic dimerization, adipic acid catalytic amination, caprolactam method and butadiene method. The acrylonitrile electrolytic dimerization method was first developed by Monsanto Company in the United States in the 1960s, and gradually developed from diaphragm electrolysis to non-diaphragm electrolysis. Due to the strong toxicity and corrosiveness of the raw material acrylonitrile, serious pollution, large electricity consumption and high production cost, it has been gradually eliminated by the market. The adipic acid catalytic amination method uses adipic acid as a raw material. Its production cost is too high due to the rising price of adipic acid and has lost its competitive advantage. It has been basically eliminated. The caprolactam method is a process for synthesizing adiponitrile using waste nylon or recycled caprolactam as raw materials. It was developed by Toray Corporation of Japan, but it is not suitable for large-scale industrial production due to the shortage of raw materials. The butadiene method is divided into butadiene chlorination cyanation method and butadiene direct cyanation method. The cyanidation of butadiene was developed by DuPont in the early 1960s. The process is complex, corrosive, and requires large investments. It also consumes a large amount of chlorine and hydrocyanic acid. It has now been replaced by DuPont's new process of direct cyanidation of butadiene. The direct cyanidation of butadiene has the advantages of simple process, short route, energy saving, environmental protection, and low cost. The process has a production share of 60-70% in the world. At present, INVISTA (formerly DuPont) and Rhodia have jointly monopolized the technology and refused to sell it to other companies.

[0004] CN 111892514 A invention provides a method for preparing adiponitrile by direct hydrocyanation of butadiene, using Lewis acid as a co-catalyst to assist Ni(0)-monodentate organic phosphine complex catalyst to catalyze isomerization reaction and secondary hydrocyanation reaction, which can effectively accelerate the reaction rate of isomerization and secondary hydrocyanation reaction. CN 113372239 A invention provides a method for preparing C5 monoolefin nitrile by direct hydrocyanation reaction of butadiene and hydrogen cyanide in the presence of Ni(0)-phosphine complex catalyst, which effectively improves the ratio of straight-chain nitrile and branched-chain nitrile, thereby saving the subsequent isomerization and separation process of adiponitrile production. However, the raw material HCN used in the above method is highly toxic and difficult to transport, which limits the extensive research of the reaction; and the phosphine ligands are all phosphite type, the ligand structure is complex, difficult to synthesize, and have strict requirements on the water content and oxygen content in the reaction system, and the reaction needs to be carried out at a higher temperature (≥100°C) and additional pressure (≥0.5MPa). Therefore, it is of great practical significance to find green and safe cyanide sources, develop stable and easy-to-synthesize phosphine ligand compounds, and prepare butadiene hydrocyanation catalysts with excellent performance. Summary of the invention

[0005] In view of the technical problems in the prior art that the raw material HCN in the process of butadiene hydrocyanation is highly toxic and difficult to transport, and that the application conditions of phosphite ligand catalysts are harsh, the preparation process of effective complex catalysts is unclear, the reaction temperature is high and additional pressure is required, the present invention provides a preparation method of a nickel complex catalyst and its application in the preparation of pentenenitrile by butadiene hydrocyanation. The nickel complex catalyst of the present invention allows the butadiene hydrocyanation reaction to be carried out under relatively mild conditions (≤80°C, ~0.1MPa), the reaction is more energy-saving and safe, the operation process is simple, and the total yield of 3 / 4-pentenenitrile and 2-methyl-3-butenenitrile is ≥90%.

[0006] In order to achieve the above object, the technical solution of the present invention is achieved as follows:

[0007] A method for preparing a nickel complex catalyst comprises the following steps: fully mixing a nickel metal salt, a bidentate phosphine ligand and a solvent under anhydrous and oxygen-free conditions, and then reacting the mixture in a sealed manner to obtain a nickel-bidentate phosphine ligand complex catalyst solution.

[0008] Further, the nickel metal salt is any one of bis-1,5-cyclooctadiene nickel, nickel acetylacetonate or nickel chloride, and the bidentate phosphine ligand has the structural formula Where R 12 , R 13 , R 22 , R 23 Each is independently an unsubstituted or substituted aromatic hydrocarbon.

[0009] Further, the bidentate phosphine ligand structural formula is

[0010]

[0011] Any one of .

[0012] Furthermore, the order of fully mixing the nickel metal salt, the bidentate phosphine ligand and the solvent is: a) fully dissolving the nickel metal salt in the solvent and then adding the bidentate phosphine ligand; or b) fully dissolving the bidentate phosphine ligand in the solvent and then adding the nickel metal salt; or c) dissolving the nickel metal salt and the bidentate phosphine ligand in the solvent respectively and then mixing them.

[0013] Furthermore, the molar ratio of the nickel metal salt to the bidentate phosphine ligand is 1:(1-5), the solvent is any one of toluene, acetonitrile, diphenyl ether, tetrahydrofuran, pyridine, N-methylpyrrolidone, dichloromethane, methanol, benzonitrile or n-hexane; the sealed reaction is carried out in a pressure-resistant tube, wherein the amount of the solvent is 4.5 mL; the sealed reaction temperature is 35-55° C., and the sealed reaction time is 5-15 min. Preferably, the sealed reaction temperature is 35° C.

[0014] Furthermore, after the nickel complex catalyst is prepared, an auxiliary agent is added, mixed, and then a sealing reaction is performed again.

[0015] Further, the auxiliary agent is any one of ZnCl2, pyridine, dimethylaminopyridine, p-hydroxypyridine, p-cyanopyridine, p-methylpyridine, benzonitrile, p-hydroxybenzonitrile, acetonitrile, 1-butyl-3-methylimidazolium hexafluorophosphate, 1-butyl-3-methylimidazolium bromide or 1-butyl-3-methylimidazolium trifluoromethanesulfonate; based on the amount of nickel metal salt added, the molar ratio of nickel metal salt to auxiliary agent is 1:(1-5), the temperature of the sealing reaction is 35-55°C, and the time of the sealing reaction is 1-6h. Preferably, the temperature of the sealing reaction is 35°C.

[0016] Furthermore, the nickel complex catalyst prepared by the above method is in a liquid homogeneous state.

[0017] A method for preparing pentenenitrile by hydrocyanation of butadiene comprises the following steps: mixing the nickel complex catalyst with alcohol under anhydrous and oxygen-free conditions, then sequentially adding butadiene and trimethylsilyl cyanide for sealing reaction, and rapidly cooling to room temperature after the reaction is completed to obtain pentenenitrile.

[0018] Furthermore, the alcohol is any one of methanol, ethanol or butanol; the molar ratio of the nickel complex catalyst, butadiene, alcohol and trimethylsilyl cyanide is 1:(110-223):110:100.

[0019] Furthermore, the sealing reaction temperature is 50 to 150° C., and the sealing reaction time is 1.5 to 5 hours.

[0020] The present invention has the following beneficial effects:

[0021] (1) The xanthene-type bidentate phosphine ligand used in the present invention has a stable structure and is easy to synthesize and apply. By regulating the complex catalytic system formed with Ni during the preparation process, the yield of pentenenitrile can reach more than 90%.

[0022] (2) The present invention clarifies the control method for catalyst preparation and studies the influence of different addition orders on the formation and reaction performance of effective complex catalysts. Therefore, the present invention provides a preparation method for obtaining an effective active complex catalyst.

[0023] (3) The reaction conditions of the present invention are mild, and the reaction is carried out at ≤80°C and without additional pressure (~0.1MPa), which can be more energy-saving and safer and easier to industrialize. DETAILED DESCRIPTION

[0024] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0025] The bidentate phosphine ligand L4 and other raw materials used in the present invention are purchased, and other bidentate phosphine ligands (such as L1\L2\L3\L5\L6) are prepared by referring to the following synthesis method, and the synthesis method is as follows:

[0026]

[0027] According to the literature, Xantphos type ligands were synthesized by the same method. At room temperature, 9,9-dimethylxanthene and TMEDA (2.5 equiv) were added to Et2O (5 mL). After the reaction mixture was cooled to 0°C, n-BuLi (1.6 M in Hexanes, 2.5 equiv.) was slowly added dropwise within 30 min and stirred at 0°C overnight. A n-hexane solution containing chlorodiphenylphosphine (2.5 equiv) was slowly added dropwise to the orange suspension for 45 min. A yellow precipitate was formed and stirred overnight. The reaction mixture was diluted with dichloromethane (6 mL) and hydrolyzed with 4 mL of brine and 1 M HCl (1:1 v / v). The aqueous phase was then removed and washed three times with dichloromethane (5 mL). The organic phase was dried over MgSO4, and the solid was left after vacuum drying, and the crystals were washed with n-hexane (3 mL). Other types of Xantphos ligands were also synthesized using the above method. The characterization data of other prepared bidentate phosphine ligands (such as L1\L2\L3\L5\L6) are as follows:

[0028] (1)9,9-dimethylxanthene-4,5-bis[bis(3,5-dimethylphenyl)phosphino](L1)

[0029] 1 H-NMR (600MHz, CDCl3, δ): 7.31 (dd, J = 7.7Hz, 2H), 6.88 (t, 2H), 6.77 (s, 4H), 6.74 (brs, 8H), 6.49 (brd, J = 7.5Hz, 2H), 2.10 (s, 24H), 1.57 (s, 6H). 13 C-NMR (151MHz, CDCl3, δ): 151.91, 136.28 (m), 136.06 (t, J = 3.5Hz), 130.96, 130.57 (t, J = 10.6Hz), 128.85, 127.19-127.09 (m), 20.32. 31 P-NMR (243MHz, CDCl3, δ): -17.37.

[0030] (2)9,9-dimethylxanthene-4,5-bis[bis(2-methylphenyl)phosphino](L2)

[0031] 1H-NMR(600MHz,CDCl3,δ):7.34(dd,J=11.2,4.7Hz,2H),7.21-7.15(m,8H),6.99-6.93(m,6H)6.59(d,J=6.4Hz,4H),6.39(dd,J=7.5,1.6Hz,2H),2.42(s,12H),1.6(s,6H). 13 C-NMR(151MHz,CDCl3,δ):151.90-151.54(m),141.74-141.30(m),133.54-133.29(m),132.30(s),131.66(s),128.92(d,J=4.9Hz),127.63(s),127.09(s),126.06(s),125.29(d,J=10.2Hz),122.33(d,J=14.8Hz),122.12,33.42,30.29,20.28(d,J=22.2Hz). 31 P-NMR(243MHz,CDCl3,δ):-31.51.

[0032] (3)9,9-dimethylxanthene-4,5bis(bis(3,5(trifluoromethyl)phenyl)phosphine)(L3)

[0033] 1 H-NMR(600MHz,CDCl3,δ):7.81(s,4H),7.53(s,8H),7.50(dd,J=7.8,13HZ,2H),7.05(t,J=7.5Hz),6.33(dd,J=7.6,1.6Hz),1.6(s,6H). 13 C-NMR(151MHz,CDCl3,δ):150.99(t,J=9.5Hz),131.38-131.18(m),131.15-130.9(m),130.49(dd,J=19.5Hz),130.15,130.02,127.20,124.06,122.46(s),120.9,119..98-120.44(m),33.71,30.6. 31 P-NMR(243MHz,CDCl3,δ):-14.51.

[0034] (4)9,9-dimethylxanthene-4,5bis(di(4(trifluoromethyl)phenyl)phosphine)(L5)

[0035] 1 H-NMR (600MHz, CDCl3, δ): 7.47-7.23 (m, 10H), 7.23-7.02 (m, 6H), 7.02 (t, J = 7.62Hz2H), 6.42 (dd, J = 7.65Hz, 2H), 1.46 (s, 6H). 13 C-NMR (151MHz, 298K, CDCl3) δ = 152.57 (t, J = 9.06Hz), 141.47 (t, J = 7.55Hz), 134.14 (t, J = 10.57Hz), 131.98, 131 .10(t,J=31.71Hz),127.51(s),125.5(q,J=3.02Hz),125.03,124.28(s),123.23,122.8,121.42,34.75,31.91. 31 P-NMR (243MHz, CDCl3, δ): -17.57.

[0036] (5)9,9-dimethylxanthene-4,5bis(di(4(methoxyl)phenyl)phosphine)(L6)

[0037] 1 H-NMR (600MHz, CDCl3, δ): 7.378 (d, J = 7.02Hz, 2H), 7.065-7.090 (m, 8H), 6.944 (t, J = 7.62Hz, 2H), 6.7 39(d,J=8.46Hz,4H),6.56(dJ=7.8Hz,2H),6.53(dd,J=7.2Hz,1.2Hz,2H),3.79(s,12H),1.64(s,6H). 13 C NMR (151MHz, CDC13, δ): 159.69, 135.27 (t, J = 43Hz), 131.83, 129.91, 128.59 ( t,J=18Hz),126.77,125.99,123.23,113.78(t,J=18Hz),54.99,34.43,31.73. 31 PNMR(243MHz,298K,CDC13,δ):-20.39.

[0038] Example 1

[0039] A method for preparing a nickel complex catalyst and its application in preparing pentenenitriles by hydrocyanation of butadiene, comprising the following steps:

[0040] (1) In a glove box, 0.0038 g Ni(COD)2 and 4.5 mL toluene were added to a pressure tube. After sufficient dissolution, 0.0355 g ligand L4 was added and stirred at 35°C for 5 min to obtain a Ni-Xantphos complex catalyst (Ni:Xantphos=1:4).

[0041] (2) Methanol, butadiene (20 wt % butadiene toluene solution) and TMSCN were added to the prepared complex catalyst solution in sequence, with the molar ratio of each compound being Ni:butadiene:methanol:TMSCN=1:180:100:100.

[0042] (3) The sealed pressure-resistant tube was placed in an 80° C. oil bath and stirred for reaction for 2.5 h. After the reaction was completed, the tube was rapidly cooled to room temperature to obtain a 3 / 4-pentenenitrile yield of 52.16% and a 2-methyl-3-butenenitrile yield of 43.53%.

[0043] Example 2

[0044] A method for preparing a nickel complex catalyst and its application in preparing pentenenitriles by hydrocyanation of butadiene, which is different from Example 1 in that: in step (1), the ligand L4 is first dissolved in toluene and then mixed with the nickel metal salt Ni(COD)2, the steps are as follows:

[0045] (1) In a glove box, 0.0355 g of ligand L4 and 4.5 mL of toluene were added to a pressure tube. After sufficient dissolution, 0.0038 g of Ni(COD)2 was added and stirred at 35°C for 5 min to obtain a Ni-Xantphos complex catalyst (Ni:Xantphos=1:4).

[0046] (2) Methanol, butadiene (20 wt % butadiene toluene solution) and TMSCN were added to the prepared complex catalyst solution in sequence, with the molar ratio of each compound being Ni:butadiene:methanol:TMSCN=1:180:100:100.

[0047] (3) The sealed pressure-resistant tube was placed in an 80° C. oil bath and stirred for reaction for 2.5 h. After the reaction was completed, the tube was rapidly cooled to room temperature to obtain a 3 / 4-pentenenitrile yield of 28.99% and a 2-methyl-3-butenenitrile yield of 39.79%.

[0048] Example 3

[0049] A method for preparing a nickel complex catalyst and its application in preparing pentenenitriles by hydrocyanation of butadiene, which is different from Example 1 in that: in step (1), the ligand L4 and the nickel metal salt Ni(COD)2 are dissolved in toluene respectively and then mixed, and the steps are as follows:

[0050] (1) In a glove box, 0.0355 g of L4 and 0.0038 g of Ni(COD)2 were dissolved in toluene, added into a pressure tube, mixed thoroughly, and stirred at 35°C for 5 min to obtain a Ni-Xantphos complex catalyst (Ni:Xantphos=1:4).

[0051] (2) Methanol, butadiene (20 wt % butadiene toluene solution) and TMSCN were added to the prepared complex catalyst solution in sequence, with the molar ratio of each compound being Ni:butadiene:methanol:TMSCN=1:180:100:100.

[0052] (3) The sealed pressure-resistant tube was placed in an 80° C. oil bath and stirred for reaction for 2.5 h. After the reaction was completed, the tube was rapidly cooled to room temperature. The yield of 3 / 4-pentenenitrile was 52.82%, and the yield of 2-methyl-3-butenenitrile was 40.46%.

[0053] Example 4

[0054] A method for preparing a nickel complex catalyst and its application in preparing pentenenitrile by hydrocyanation of butadiene, which is different from Example 1 in that: in step (1), nickel metal salt Ni(COD)2 is dissolved in toluene and then mixed with ligand L4, the steps are as follows:

[0055] (1) In a glove box, 0.0038 g Ni(COD)2 and 4.5 mL acetonitrile were added to a pressure tube. After sufficient dissolution, 0.0355 g ligand L4 was added and stirred at 35°C for 5 min to obtain a Ni-Xantphos complex catalyst (Ni:Xantphos=1:4).

[0056] (2) Methanol, butadiene (20 wt % butadiene toluene solution) and TMSCN were added to the prepared complex catalyst solution in sequence, with the molar ratio of each compound being Ni:butadiene:methanol:TMSCN=1:180:100:100.

[0057] (3) The sealed pressure-resistant tube was placed in an 80° C. oil bath and stirred for reaction for 2.5 h. After the reaction was completed, the tube was rapidly cooled to room temperature to obtain a 3 / 4-pentenenitrile yield of 26.39% and a 2-methyl-3-butenenitrile yield of 23.94%.

[0058] Example 5

[0059] A method for preparing a nickel complex catalyst and its application in preparing pentenenitriles by hydrocyanation of butadiene, which is different from Example 1 in that the amount of butadiene is reduced in step (2), and the steps are as follows:

[0060] (1) In a glove box, 0.0038 g Ni(COD)2 and 4.5 mL toluene were added to a pressure tube. After sufficient dissolution, 0.0355 g ligand L4 was added and stirred at 35°C for 5 min to obtain a Ni-Xantphos complex catalyst (Ni:Xantphos=1:4).

[0061] (2) Methanol, butadiene (20 wt % butadiene toluene solution) and TMSCN were added to the prepared complex catalyst solution in sequence, with the molar ratio of each compound being Ni:butadiene:methanol:TMSCN=1:110:100:100.

[0062] (3) The sealed pressure-resistant tube was placed in an 80° C. oil bath and stirred for reaction for 2.5 h. After the reaction was completed, the tube was rapidly cooled to room temperature. The yield of 3 / 4-pentenenitrile was 27.03%, and the yield of 2-methyl-3-butenenitrile was 34.22%.

[0063] Example 6

[0064] A method for preparing a nickel complex catalyst and its application in preparing pentenenitrile by hydrocyanation of butadiene, which is different from Example 5 in that: in step (1), the amount of ligand L4 is increased so that Ni:Xantphos in the catalyst is 1:1, and the steps are as follows:

[0065] (1) In a glove box, 0.0038 g Ni(COD)2 and 4.5 mL toluene were added to a pressure tube. After sufficient dissolution, 0.0089 g ligand L4 was added and stirred at 35°C for 5 min to obtain a Ni-Xantphos complex catalyst (Ni:Xantphos=1:1).

[0066] (2) Methanol, butadiene (20 wt % butadiene toluene solution) and TMSCN were added to the prepared complex catalyst solution in sequence, with the molar ratio of each compound being Ni:butadiene:methanol:TMSCN=1:110:100:100.

[0067] (3) The sealed pressure-resistant tube was placed in an 80° C. oil bath with stirring for reaction for 2.5 h. After the reaction was completed, the tube was rapidly cooled to room temperature to obtain 3 / 4-pentenenitrile with a yield of 11.56% and 2-methyl-3-butenenitrile with a yield of 14.80%.

[0068] Example 7

[0069] A method for preparing a nickel complex catalyst and its application in preparing pentenenitriles by hydrocyanation of butadiene, which is different from Example 5 in that the temperature of the oil bath is lowered in step (3), and the steps are as follows:

[0070] (1) In a glove box, 0.0038 g Ni(COD)2 and 4.5 mL toluene were added to a pressure tube. After sufficient dissolution, 0.0355 g ligand L4 was added and stirred at 35°C for 5 min to obtain a Ni-Xantphos complex catalyst (Ni:Xantphos=1:4).

[0071] (2) Methanol, butadiene (20 wt % butadiene toluene solution) and TMSCN were added to the prepared complex catalyst solution in sequence, with the molar ratio of each compound being Ni:butadiene:methanol:TMSCN=1:110:100:100.

[0072] (3) The sealed pressure-resistant tube was placed in a 50° C. oil bath and stirred for reaction for 2.5 h. After the reaction was completed, the tube was rapidly cooled to room temperature to obtain a 3 / 4-pentenenitrile yield of 7.64% and a 2-methyl-3-butenenitrile yield of 10.13%.

[0073] Example 8

[0074] A method for preparing a nickel complex catalyst and its application in preparing pentenenitriles by hydrocyanation of butadiene, which is different from Example 5 in that the oil bath time in step (3) is shortened, and the steps are as follows:

[0075] (1) In a glove box, 0.0038 g Ni(COD)2 and 4.5 mL toluene were added to a pressure tube. After sufficient dissolution, 0.0355 g ligand L4 was added and stirred at 35°C for 5 min to obtain a Ni-Xantphos complex catalyst (Ni:Xantphos=1:4).

[0076] (2) Methanol, butadiene (20 wt % butadiene toluene solution) and TMSCN were added to the prepared complex catalyst solution in sequence, with the molar ratio of each compound being Ni:butadiene:methanol:TMSCN=1:110:100:100.

[0077] (3) The sealed pressure-resistant tube was placed in an 80° C. oil bath and stirred for reaction for 0.5 h. After the reaction was completed, the tube was rapidly cooled to room temperature to obtain a 3 / 4-pentenenitrile yield of 9.12% and a 2-methyl-3-butenenitrile yield of 10.88%.

[0078] Example 9

[0079] A method for preparing a nickel complex catalyst and its application in preparing pentenenitriles by hydrocyanation of butadiene, which is different from Example 1 in that: in step (1), the amount of ligand is reduced, and an auxiliary agent, p-hydroxybenzonitrile (HOPhCN), is added, and the steps are as follows:

[0080] (1) In a glove box, 0.0038 g Ni(COD)2 and 4.5 mL toluene were added to a pressure tube, and after fully dissolving, 0.0178 g ligand L4 was added, and stirred at 35°C for 5 min to obtain a Ni-Xantphos complex catalyst (Ni:Xantphos=1:2). 0.0085 g p-hydroxybenzonitrile (HOPhCN) was added to the above mixture solution, and after stirring at 35°C for 5 h, a Ni-bidentate phosphine ligand-auxiliary agent complex catalyst (Ni:Xantphos:HOPhCN=1:2:5) was obtained.

[0081] (2) Methanol, butadiene (20 wt % butadiene toluene solution) and TMSCN were added to the prepared complex catalyst solution in sequence, with the molar ratio of each compound being Ni:butadiene:methanol:TMSCN=1:180:100:100.

[0082] (3) The sealed pressure-resistant tube was placed in an 80° C. oil bath and stirred for reaction for 2.5 h. After the reaction was completed, the tube was rapidly cooled to room temperature. The yield of 3 / 4-pentenenitrile was 33.97%, and the yield of 2-methyl-3-butenenitrile was 42.25%.

[0083] Example 10

[0084] A method for preparing a nickel complex catalyst and its application in preparing pentenenitriles by hydrocyanation of butadiene, which is different from Example 9 in that: in step (1), ZnCl2 is used as an auxiliary agent, and the amount of the auxiliary agent added is different; in step (2), the stirring time is shortened, and the steps are as follows:

[0085] (1) In a glove box, 0.0038 g Ni(COD)2 and 4.5 mL toluene were added to a pressure tube, and after fully dissolving, 0.0178 g ligand L4 was added, and stirred at 35°C for 5 min to obtain a Ni-Xantphos complex catalyst (Ni:Xantphos=1:2). 0.0038 g ZnCl2 was added to the above mixture solution, and after stirring at 35°C for 5 h and stirring evenly, a Ni-bidentate phosphine ligand-promoter complex catalyst (Ni:Xantphos:ZnCl2=1:2:5) was obtained.

[0086] (2) Methanol, butadiene (20 wt % butadiene toluene solution) and TMSCN were added to the prepared complex catalyst solution in sequence, with the molar ratio of each compound being Ni:butadiene:methanol:TMSCN=1:180:100:100.

[0087] (3) The sealed pressure-resistant tube was placed in an 80° C. oil bath and stirred for reaction for 2.5 h. After the reaction was completed, the tube was rapidly cooled to room temperature to obtain a 3 / 4-pentenenitrile yield of 31.36% and a 2-methyl-3-butenenitrile yield of 39.26%.

[0088] Embodiment 11

[0089] A method for preparing a nickel complex catalyst and its application in preparing pentenenitriles by hydrocyanation of butadiene, which is different from Example 5 in that a reducing agent, zinc powder, is added in step (1), and the steps are as follows:

[0090] (1) In a glove box, 0.0038 g of Ni(acac)2 and 4.5 mL of toluene were added to a pressure tube. After sufficient dissolution, 0.0355 g of L4 and 0.0012 g of reducing agent zinc powder were added, and the mixture was stirred at 35°C for 20 min to obtain a Ni-Xantphos complex catalyst (Ni:Xantphos=1:4).

[0091] (2) Methanol, butadiene (20 wt % butadiene toluene solution) and TMSCN were added to the prepared complex catalyst solution in sequence, with the molar ratio of each compound being Ni:butadiene:methanol:TMSCN=1:110:100:100.

[0092] (3) The sealed pressure-resistant tube was placed in an 80° C. oil bath and stirred for reaction for 2.5 h. After the reaction was completed, the tube was quickly cooled to room temperature. The yield of pentenenitrile was 0%.

[0093] Example 12

[0094] A method for preparing a nickel complex catalyst and its application in preparing pentenenitriles by hydrocyanation of butadiene, which is different from Example 1 in that the ligand in step (1) is L5, and the steps are as follows:

[0095] (1) In a glove box, 0.0038 g Ni(COD)2 and 4.5 mL toluene were added to a pressure tube. After sufficient dissolution, 0.0464 g ligand L5 was added and stirred at 35°C for 5 min to obtain a Ni-L5 complex catalyst (Ni:L5=1:4).

[0096] (2) Methanol, butadiene (20 wt % butadiene toluene solution) and TMSCN were added to the prepared complex catalyst solution in sequence, with the molar ratio of each compound being Ni:butadiene:methanol:TMSCN=1:180:100:100.

[0097] (3) The sealed pressure-resistant tube was placed in an 80° C. oil bath with stirring for reaction for 2.5 h. After the reaction was completed, the tube was rapidly cooled to room temperature to obtain a 3 / 4-pentenenitrile yield of 45.76% and a 2-methyl-3-butenenitrile yield of 37.48%.

[0098] Embodiment 13

[0099] A method for preparing a nickel complex catalyst and its application in preparing pentenenitriles by hydrocyanation of butadiene, which is different from Example 5 in that the oil bath temperature is increased in step (3), and the steps are as follows:

[0100] (1) In a glove box, 0.0038 g Ni(COD)2 and 4.5 mL toluene were added to a pressure tube. After sufficient dissolution, 0.0355 g ligand L4 was added and stirred at 35°C for 5 min to obtain a Ni-L4 complex catalyst (Ni:L4=1:4).

[0101] (2) Methanol, butadiene (20 wt % butadiene toluene solution) and TMSCN were added to the prepared complex catalyst solution in sequence, with the molar ratio of each compound being Ni:butadiene:methanol:TMSCN=1:110:100:100.

[0102] (3) The sealed pressure-resistant tube was placed in a 150° C. oil bath and stirred for reaction for 2.5 h. After the reaction was completed, the tube was rapidly cooled to room temperature to obtain a 3 / 4-pentenenitrile yield of 28.68% and a 2-methyl-3-butenenitrile yield of 26.73%.

[0103] Embodiment 14

[0104] A method for preparing a nickel complex catalyst and its application in preparing pentenenitriles by hydrocyanation of butadiene, which is different from Example 1 in that the stirring temperature in steps (1) and (2) is changed, and the steps are as follows:

[0105] (1) In a glove box, 0.0038 g Ni(COD)2 and 4.5 mL toluene were added to a pressure tube. After sufficient dissolution, 0.0355 g ligand L4 was added and stirred at 45°C for 5 min to obtain a Ni-Xantphos complex catalyst (Ni:Xantphos=1:4).

[0106] (2) Methanol, butadiene (20 wt % butadiene toluene solution) and TMSCN were added to the prepared complex catalyst solution in sequence, with the molar ratio of each compound being Ni:butadiene:methanol:TMSCN=1:180:100:100.

[0107] (3) The sealed pressure-resistant tube was placed in an 80° C. oil bath and stirred for reaction for 2.5 h. After the reaction was completed, the tube was rapidly cooled to room temperature to obtain a 3 / 4-pentenenitrile yield of 42.12% and a 2-methyl-3-butenenitrile yield of 49.45%.

[0108] Embodiment 15

[0109] A method for preparing a nickel complex catalyst and its application in preparing pentenenitriles by hydrocyanation of butadiene, which is different from Example 1 in that the stirring temperature in steps (1) and (2) is changed, and the steps are as follows:

[0110] (1) In a glove box, 0.0038 g Ni(COD)2 and 4.5 mL toluene were added to a pressure tube. After sufficient dissolution, 0.0355 g ligand L4 was added and stirred at 55°C for 5 min to obtain a Ni-Xantphos complex catalyst (Ni:Xantphos=1:4).

[0111] (2) Methanol, butadiene (20 wt % butadiene toluene solution) and TMSCN were added to the prepared complex catalyst solution in sequence, with the molar ratio of each compound being Ni:butadiene:methanol:TMSCN=1:180:100:100.

[0112] (3) The sealed pressure-resistant tube was placed in an 80° C. oil bath and stirred for reaction for 2.5 h. After the reaction was completed, the tube was rapidly cooled to room temperature to obtain a 3 / 4-pentenenitrile yield of 23.66% and a 2-methyl-3-butenenitrile yield of 32.65%.

[0113] Example 16

[0114] A method for preparing a nickel complex catalyst and its application in preparing pentenenitriles by hydrocyanation of butadiene, which is different from Example 1 in that the stirring time in step (3) is changed, and the steps are as follows:

[0115] (1) In a glove box, 0.0038 g Ni(COD)2 and 4.5 mL toluene were added to a pressure tube. After sufficient dissolution, 0.0355 g ligand L4 was added and stirred at 35°C for 5 min to obtain a Ni-Xantphos complex catalyst (Ni:Xantphos=1:4).

[0116] (2) Methanol, butadiene (20 wt % butadiene toluene solution) and TMSCN were added to the prepared complex catalyst solution in sequence, with the molar ratio of each compound being Ni:butadiene:methanol:TMSCN=1:180:100:100.

[0117] (3) The sealed pressure-resistant tube was placed in an 80° C. oil bath and stirred for reaction for 5 h. After the reaction was completed, the tube was rapidly cooled to room temperature to obtain a 3 / 4-pentenenitrile yield of 32.4% and a 2-methyl-3-butenenitrile yield of 26.42%.

[0118] Embodiment 17

[0119] A method for preparing a nickel complex catalyst and its application in preparing pentenenitriles by hydrocyanation of butadiene, which is different from Example 9 in that no auxiliary agent is added in step (1), and the steps are as follows:

[0120] (1) In a glove box, 0.0038 g Ni(COD)2 and 4.5 mL toluene were added to a pressure tube. After sufficient dissolution, 0.0178 g ligand L4 was added and stirred at 35°C for 5 min to obtain a Ni-Xantphos complex catalyst (Ni:Xantphos=1:2).

[0121] (2) Methanol, butadiene (20 wt % butadiene toluene solution) and TMSCN were added to the prepared complex catalyst solution in sequence, with the molar ratio of each compound being Ni:butadiene:methanol:TMSCN=1:180:100:100.

[0122] (3) The sealed pressure-resistant tube was placed in an 80° C. oil bath with stirring for reaction for 2.5 h. After the reaction was completed, the tube was rapidly cooled to room temperature to obtain a 3 / 4-pentenenitrile yield of 20.7% and a 2-methyl-3-butenenitrile yield of 27%.

[0123] Embodiment 18

[0124] A method for preparing a nickel complex catalyst and its application in preparing pentenenitriles by hydrocyanation of butadiene, which is different from Example 1 in that: in step (1), the amount of ligand is reduced, and an auxiliary agent, p-hydroxybenzonitrile (HOPhCN), is added, and the steps are as follows:

[0125] (1) In a glove box, 0.0038 g Ni(COD)2 and 4.5 mL toluene were added to a pressure tube, and after fully dissolving, 0.0178 g ligand L4 was added, and stirred at 35°C for 5 min to obtain a Ni-Xantphos complex catalyst (Ni:Xantphos=1:2). 0.0085 g p-dimethylaminopyridine was added to the above mixture solution and stirred at 35°C for 5 h to obtain a Ni-bidentate phosphine ligand-auxiliary agent complex catalyst (Ni:Xantphos:p-dimethylaminopyridine=1:2:5).

[0126] (2) Methanol, butadiene (20 wt % butadiene toluene solution) and TMSCN were added to the prepared complex catalyst solution in sequence, with the molar ratio of each compound being Ni:butadiene:methanol:TMSCN=1:180:100:100.

[0127] (3) The sealed pressure-resistant tube was placed in an 80° C. oil bath and stirred for reaction for 2.5 h. After the reaction was completed, the tube was rapidly cooled to room temperature to obtain a 3 / 4-pentenenitrile yield of 31.61% and a 2-methyl-3-butenenitrile yield of 22.70%.

[0128] By studying the different addition orders of substances in the preparation of nickel-bidentate phosphine ligand complex catalyst solution, it is found that compared with Example 1, Example 2, and Example 3, Example 1: adding Ni(COD)2 and toluene to the pressure tube, adding ligand L4 after fully dissolving and Example 3: fully dissolving L4 and Ni(COD)2 in toluene before mixing and reacting have better effects. Compared with Example 1, in Example 4, the solvent toluene is replaced with acetonitrile. Since acetonitrile has a large polarity, the reaction yield decreases, and a non-polar solvent will help the reaction.

[0129] Compared with Example 1, in Example 5, when the butadiene:TMSCN ratio was reduced from 180:100 to 110:100, the reaction yield decreased. When an excess of butadiene was added, the amount of butadiene in the liquid phase increased during the reaction, which facilitated the reaction.

[0130] Compared with Example 1, when the Ni:Xantphos ratio in Example 6 was reduced from 1:4 to 1:1, the amount of Xantphos added was reduced, and Ni(0) could not be fully protected, causing it to be poisoned and inactivated, resulting in a decrease in the reaction yield.

[0131] Compared with Example 5, Example 7 and Example 13 were reacted at 50° C. and 150° C., respectively. Too low or too high a temperature would lead to a decrease in the reaction yield.

[0132] Compared with Example 5, the reaction time in Example 8 was reduced to 0.5 h, and the reaction yield decreased.

[0133] Compared with Example 1, in Example 9 and Example 10, auxiliary agents p-hydroxybenzonitrile and ZnCl2 were added to adjust the normal-iso ratio of the reaction product, and the reaction yield was reduced as a whole and the normal-iso ratio of the reaction could not be adjusted. However, compared with Example 17, after adding the auxiliary agents, the reaction yields of Example 9 and Example 10 were increased as a whole and the normal-iso ratio was improved to a certain extent.

[0134] Compared with Example 5, Example 11 uses Ni(acac)2 as the nickel source. Due to the low reaction temperature, the reducing agent Zn powder cannot reduce Ni(II) to Ni(0) during the reaction, so the reaction yield is 0.

[0135] Compared with Example 1, in Example 12, L5 is used as the ligand. When toluene is taken by p-CF3, the steric hindrance of the reaction is increased, and the reaction ratio can be adjusted, but the overall reaction yield is reduced.

[0136] Compared with Example 1, in Example 14 and Example 15, as the stirring temperature increases, the deactivation rate of the Ni catalyst is accelerated and the reaction yield is reduced.

[0137] Compared with Example 1, in Example 16, as the reaction time was prolonged, the product underwent a hydrogenation reaction to generate valeronitrile, resulting in a decrease in the reaction yield.

[0138] Compared with Example 17, after adding the auxiliary agent in Example 18, the reaction yield is increased overall, and the normal-to-iso ratio is significantly improved, thus verifying the purpose of using the auxiliary agent to adjust the normal-to-iso ratio of pentenenitriles.

[0139] The present invention proposes to produce HCN in situ using alcohol and TMSCN as raw materials; using xanthene-type bidentate phosphine as ligand for catalyst preparation process; obtaining Ni-bidentate phosphine ligand complex catalyst by regulation, and applying it to the process of preparing pentenenitrile by hydrocyanation of butadiene. The in situ production of HCN using alcohol and TMSCN as raw materials has the advantages of being green, safe, and easy to use. The xanthene-type ligand has the advantages of simple structure, stable properties, and easy synthesis. The catalyst allows the hydrocyanation reaction of butadiene to be carried out under relatively mild conditions (≤80°C, ~0.1MPa), the reaction is more energy-saving and safe, the operation process is simple, and the total yield of 3 / 4-pentenenitrile and 2-methyl-3-butenenitrile is ≥90%.

[0140] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a nickel complex catalyst, characterized in that: Under anhydrous and oxygen-free conditions, nickel metal salt, bidentate phosphine ligand and solvent are fully mixed, and then sealed for reaction to obtain nickel complex catalyst I.

2. The method for preparing a nickel complex catalyst according to claim 1, characterized in that: The nickel metal salt is any one of bis-1,5-cyclooctadiene nickel, nickel acetylacetonate or nickel chloride, and the structural formula of the bidentate phosphine ligand is Where R 12 , R 13 , R 22 , R 23 Each is independently an unsubstituted or substituted aromatic hydrocarbon.

3. The method for preparing the nickel complex catalyst according to claim 2, characterized in that: The bidentate phosphine ligand structural formula is Any one of .

4. The method for preparing the nickel complex catalyst according to claim 3, characterized in that: The order of fully mixing the nickel metal salt, the bidentate phosphine ligand and the solvent is: a) fully dissolving the nickel metal salt in the solvent and then adding the bidentate phosphine ligand; or b) fully dissolving the bidentate phosphine ligand in the solvent and then adding the nickel metal salt; or c) dissolving the nickel metal salt and the bidentate phosphine ligand in the solvent respectively and then mixing them.

5. The method for preparing the nickel complex catalyst according to any one of claims 1 to 4, characterized in that: The molar ratio of the nickel metal salt and the bidentate phosphine ligand is 1:(1-5), the solvent is any one of toluene, acetonitrile, diphenyl ether, tetrahydrofuran, pyridine, N-methylpyrrolidone, dichloromethane, methanol, benzonitrile or n-hexane; the sealing reaction temperature is 35-55° C., and the sealing reaction time is 5-15 min.

6. The method for preparing the nickel complex catalyst according to any one of claims 1 to 4, characterized in that: After the nickel complex catalyst I is prepared, an auxiliary agent is added, mixed, and then sealed and reacted again to obtain the nickel complex catalyst II.

7. The method for preparing the nickel complex catalyst according to claim 6, characterized in that: The auxiliary agent is any one of ZnCl2, pyridine, dimethylaminopyridine, p-hydroxypyridine, p-cyanopyridine, p-methylpyridine, benzonitrile, p-hydroxybenzonitrile, acetonitrile, 1-butyl-3-methylimidazolium hexafluorophosphate, 1-butyl-3-methylimidazolium bromide or 1-butyl-3-methylimidazolium trifluoromethanesulfonate; based on the amount of nickel metal salt added, the molar ratio of the nickel metal salt to the auxiliary agent is 1:(1-5), the temperature of the sealing reaction is 35-55°C, and the time of the sealing reaction is 1-6h.

8. A nickel complex catalyst prepared by the method of any one of claims 1 to 4 or 7.

9. A method for preparing pentenenitriles by hydrocyanation of butadiene, characterized in that: Under anhydrous and oxygen-free conditions, the nickel complex catalyst according to claim 8 is used as a catalyst, mixed with alcohol, and then butadiene and trimethylsilyl cyanide are added in sequence for sealing reaction, and after the reaction is completed, it is quickly cooled to room temperature to obtain pentenenitrile.

10. The method for preparing pentenenitriles by hydrocyanation of butadiene according to claim 9, characterized in that: The alcohol is any one of methanol, ethanol or butanol; the molar ratio of the nickel complex catalyst, butadiene, alcohol and trimethylsilyl cyanide is 1:(110-223):110:100; the sealing reaction temperature is 50-150°C, and the sealing reaction time is 1.5-5h.

Citation Information

Patent Citations

  • Method for preparing 3-pentenenitrile

    CN109721508A

  • Preparation method of alkyl nitrile compound

    CN111484472A

  • Method for preparing adiponitrile by direct hydrocyanation of butadiene

    CN111892514A

  • Method for preparing C5 mono-olefinenitrile through reaction of 1, 3-butadiene and hydrogen cyanide

    CN113372239A

  • Phosphonite ligands and their use in hydrocyanation

    US20030195372A1