Preparation method of self-cleaning glass coating precursor solution

Through the treatment of DL-homocysteine ​​sulfolide hydrochloride and NaHCO3 solution, combined with the reaction of acrylochloride and heptadecyl ester, an efficient self-cleaning glass coating precursor solution was generated, solving the existing coating The layer material has a smooth and complex preparation problem, achieving efficient hydrophobic and oleophobic properties and simplified processes.

CN118930733AInactive Publication Date: 2024-11-12HAIAN INST OF HIGH TECH RES NANJING UNIV

Patent Information

Application Number
CN202411120210.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing self-cleaning glass coating materials such as PDMS have a smooth feeling due to the flexibility of the molecular chain, which affects the user experience, and the preparation process is complicated, making it difficult to achieve industrial application.

Method used

DL-homocysteine ​​sulfolide hydrochloride and NaHCO3 solution were stirred, acryloyl chloride and saturated brine were added and extracted by ethyl acetate to obtain TLaAm as a white solid, then filtered in dry acetone and 1H,1H acrylic acid was added. ,2H,2H-heptafluoride ester and photoinitiator react at room temperature to form the glass coating precursor solution TTFP.

Benefits of technology

The prepared self-cleaning glass coating precursor solution has efficient protection and cleaning performance, simplifies the process flow, reduces costs, and is suitable for industrial applications of large-area glass coatings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930733A_ABST
    Figure CN118930733A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a self-cleaning glass coating precursor solution, and is characterized in that the preparation method comprises the following steps: 1) dissolving DL-homocysteine thiolactone hydrochloride in a NaHCO3 solution, and uniformly stirring; 2) adding acryloyl chloride into the stirred solution, and stirring overnight at room temperature; 3) adding saturated salt water into the overnight solution for dilution, and extracting with ethyl acetate; the preparation method comprises the following steps of 1, extracting a glass coating precursor solution, 2, extracting the glass coating precursor solution, 4, drying and filtering the glass coating precursor solution through MgSO4, and carrying out recrystallization to collect a white solid product TLaAm, 5, dissolving TLaAm in dry acetone and carrying out filtration and purification through a filter membrane, 6, adding acrylic acid 1H, 1H, 2H, 2H-heptadecafluorodecyl and a 184 photoinitiator into the purified TLaAm solution and carrying out stirring, and 7, carrying out a reaction under an LED UV lamp at a room temperature after stirring to obtain the glass coating precursor solution.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of self-cleaning coatings, and in particular to a method for preparing a self-cleaning glass coating precursor solution. Background Art

[0002] Glass coatings can also be divided according to their specific functions. For example, transparent conductive coatings can make glass conductive and are widely used in electronic displays, smart glass, and solar panels. There are also heat-insulating coatings, including metal oxides, metal films, etc. These coatings can effectively reduce the amount of external heat entering the room, thereby reducing the indoor temperature and achieving the goal of energy saving and consumption reduction. Another common coating in life is UV protection, which is specifically used to block and absorb ultraviolet rays to protect human health and furniture and objects from ultraviolet damage.

[0003] Self-cleaning coatings have always been the research focus in the field of surface chemistry. Self-cleaning coatings can make the glass surface form a super-hydrophobic or super-oleophobic surface, effectively preventing dust and dirt from sticking and making it easier to clean. Self-cleaning coatings have always been the research focus in the field of surface chemistry. High light transmittance, super-hydrophobic and oleophobic functions are crucial for application on glass surfaces, and there is a huge demand for their application in the fields of construction, automobiles, decoration, etc.

[0004] The widely used polydimethylsiloxane (PDMS) coating exhibits liquid properties due to the flexibility of the grafted chain, which can repel water-based and oily pollutants. However, the larger molecular chain of PDMS makes the surface slippery, affecting the user experience. The use of fluorinated epoxy can overcome the above shortcomings while improving the surface touch. Summary of the invention

[0005] The purpose of the present invention is to provide a method for preparing a self-cleaning glass coating precursor solution. The method of the present invention has mild conditions, low cost, simplicity and reliability. The prepared self-cleaning glass precursor solution has the advantages of good protective effect and strong cleaning ability, so as to solve the shortcomings mentioned in the above background technology.

[0006] To achieve the above object, the present invention provides the following technical solutions: The present invention provides a method for preparing a self-cleaning glass coating precursor solution, comprising the following steps: (1) Dissolve DL-homocysteine ​​thiolactone hydrochloride in NaHCO 3 The solution was stirred evenly; (2) Add acryloyl chloride to the stirred solution and stir at room temperature overnight; (3) The overnight solution was diluted with saturated brine and extracted with ethyl acetate; (4) After extraction, MgSO 4After drying and filtration, the white solid product TLaAm was collected by recrystallization; (5) Dissolve TLaAm in dry acetone and purify it by filtering with a filter membrane; (6) Add 1H, 1H, 2H, 2H-heptadecafluorodecyl acrylate and 184 photoinitiator to the purified TLaAm solution and stir; (7) After stirring, the mixture is reacted under an LED UV lamp at room temperature, and the resulting solution is the glass coating precursor solution TTFP solution.

[0007] Preferably, the DL-homocysteine ​​thiolactone hydrochloride in step (1) is reacted with NaHCO 3 The solution dosage ratio is (10~12)g: (180~220)ml.

[0008] Preferably, the NaHCO in step (1) 3 The solution includes NaHCO 3 A mixture of water and dioxane, with a volume ratio of water to dioxane of 1:1, NaHCO 3 The dosage for the mixture of water and dioxane is (15~20) g: (180~220) ml.

[0009] Preferably, in step (1), the stirring temperature is between -5°C and 10°C, and the stirring time is between 20 min and 40 min.

[0010] Preferably, in step (2), the ratio of the solution obtained in step 1) to acryloyl chloride is (190-250) ml: (10-15) g.

[0011] Preferably, in step (3), the volume ratio of the solution obtained in step (2) to the saturated brine is 1:1, and the number of extractions is 3-6 times.

[0012] Preferably, in step (5), the ratio of TLaAm to dry acetone is (1-5) g: (35-45) g, and the pore size of the filter membrane is 0.20 μm-0.24 μm.

[0013] Preferably, in step (6), the ratio of 1H,1H,2H,2H-heptadecafluorodecyl acrylate to 184 photoinitiator is (3-6) g: (0.1-0.2) g, and the stirring time is 30 min-50 min.

[0014] Preferably, in step (7), the power of the LED UV lamp is 300w~500w, and the reaction time is 20min~40min.

[0015] The present invention provides a self-cleaning glass coating precursor solution prepared by the method described in the above technical solution.

[0016] Compared with the prior art, the present invention has the following advantages and effects: The method for preparing the glass coating precursor solution of the present invention is simple and convenient, does not require cumbersome processes, is expected to become an industrial processing method, and provides the possibility of industrialization of large-area glass coatings.

[0017] The invention has a protective effect on the glass substrate, has high self-cleaning performance, and has good hydrophobic and oleophobic properties. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0019] Figure 1 This is a schematic diagram of steps 1-4 in Example 1; Figure 2 This is a schematic diagram of steps 5-7 in Example 1; Figure 3 The self-cleaning performance test of the glass coating precursor solution prepared in Example 3 on the glass coating surface; Figure 4 This is a photo of the coated slide after curing. DETAILED DESCRIPTION

[0020] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0021] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the present invention is further described in detail below with reference to the accompanying drawings and specific embodiments. Example 1

[0022] A method for preparing a self-cleaning glass coating precursor solution comprises the following steps: Step 1: dissolving 10 g of DL-homocysteine ​​thiolactone hydrochloride in 200 mL of NaHCO 3 Solution (16 g NaHCO 3 , water / dioxane, volume 1:1), and stirred at 0°C for 30 min.

[0023] Step 2: Add 12 g of acryloyl chloride and stir at room temperature overnight.

[0024] Step 3: After diluting with 200 mL of saturated brine, extract with ethyl acetate four times.

[0025] Step 4: The organic phase was purified by MgSO 4 After drying and filtration, the white solid product TLaAm was collected by recrystallization.

[0026] Step 5: Dissolve TLaAm in 40 g dry acetone and purify it by filtering with a 0.22 μm filter membrane.

[0027] Step 6: Add 5.18 g of 1H, 1H, 2H, 2H-heptadecafluorodecyl ester and 0.15 g of 184 photoinitiator to the TLaAm solution and stir for 30 min. Step 7: React under 400w LED UV light at room temperature for 30 minutes. The resulting solution is the glass coating precursor solution TTFP solution. Example 2

[0028] The difference from Example 1 is that the homocysteine ​​thiolactone hydrochloride in step 1 is reacted with NaHCO 3 Solution (16 g NaHCO 3 , water / dioxane, volume 1:1) in a ratio of 11 g and 200 ml respectively, and the remaining steps are the same as in Example 1. Example 3

[0029] The difference from Example 1 is that the homocysteine ​​thiolactone hydrochloride in step 1 is reacted with NaHCO 3 Solution (16 g NaHCO 3 , water / dioxane, volume 1:1) in a ratio of 12 g and 200 ml respectively, and the remaining steps are the same as in Example 1.

[0030] The invention has a protective effect on the glass substrate, has high self-cleaning performance, and has good hydrophobic and oleophobic properties.

[0031] The self-cleaning glass precursor solutions prepared in Examples 1, 2, and 3 were brush-coated on glass slides, respectively. Figure 4 It can be seen that as the transparency of the coating increases, it plays a better protective role.

[0032] Figure 3 Using wool scraps as simulated pollutants, the scraps were tilted on the surface of the solution prepared in Example 3, and water drops were squeezed out with a dropper to slide down from the top. It can be seen that when the water droplets pass through the surface, they can take away the hydrophilic wool scraps pollutants while sliding down. After the entire self-cleaning process, the pollutants on the surface were completely removed without any residual stains. The cleaning performance is relatively efficient.

[0033] The above shows and describes the basic principles and main features of the present invention and the advantages of the present invention. It should be understood by those skilled in the art that the present invention is not limited to the above embodiments. The above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.

Claims

1. A method for preparing a self-cleaning glass coating precursor solution, characterized in that: The preparation method comprises the following steps: (1) Dissolve DL-homocysteine ​​thiolactone hydrochloride in NaHCO3 solution and stir evenly; (2) Add acryloyl chloride to the stirred solution and stir at room temperature overnight; (3) The overnight solution was diluted with saturated brine and extracted with ethyl acetate; (4) After extraction, the white solid product TLaAm was collected by recrystallization after drying with MgSO4 and filtering; (5) Dissolve TLaAm in dry acetone and purify it by filtering with a filter membrane; (6) Add 1H, 1H, 2H, 2H-heptadecafluorodecyl acrylate and 184 photoinitiator to the purified TLaAm solution and stir; (7) After stirring, the mixture is reacted under an LED UV lamp at room temperature, and the resulting solution is the glass coating precursor solution TTFP solution.

2. The method for preparing the self-cleaning glass coating precursor solution according to claim 1, characterized in that: The ratio of DL-homocysteine ​​thiolactone hydrochloride to NaHCO3 solution in step (1) is (10-12) g: (180-220) ml.

3. The method for preparing the self-cleaning glass coating precursor solution according to claim 1, characterized in that: The NaHCO3 solution in step (1) includes a mixture of NaHCO3, water and dioxane, the volume ratio of water to dioxane is 1:1, and the amount of the mixture of NaHCO3, water and dioxane is (15-20) g: (180-220) ml.

4. The method for preparing the self-cleaning glass coating precursor solution according to claim 1, characterized in that: In step (1), the stirring temperature is between -5°C and 10°C, and the stirring time is between 20min and 40min.

5. The method for preparing the self-cleaning glass coating precursor solution according to claim 1, characterized in that: In step (2), the ratio of the solution obtained in step 1) to acryloyl chloride is (190-250) ml: (10-15) g.

6. The method for preparing the self-cleaning glass coating precursor solution according to claim 1, characterized in that: In step (3), the volume ratio of the solution obtained in step 2) to the saturated brine is 1:1, and the number of extractions is 3-6 times.

7. The method for preparing the self-cleaning glass coating precursor solution according to claim 1, characterized in that: In step (5), the usage ratio of TLaAm to dry acetone is (1-5) g: (35-45) g, and the pore size of the filter membrane is 0.20 μm-0.24 μm.

8. The method for preparing the self-cleaning glass coating precursor solution according to claim 1, characterized in that: Step (6) The ratio of 1H,1H,2H,2H-heptadecafluorodecyl acrylate to 184 photoinitiator is (3-6) g: (0.1-0.2) g, and the stirring time is 30 min-50 min.

9. The method for preparing the self-cleaning glass coating precursor solution according to claim 1, characterized in that: Step (7) LED UV lamp power 300w~500w, reaction time 20min~40min.

Citation Information

Patent Citations

  • Method for preparing perfluor alkyl ethide phosphite ester

    CN101445515A

  • Superhydrophobic visible light photocatalytic self-cleaning coating layer and preparation method thereof

    CN108003710A

  • Preparation method of reproducible double-self-cleaning super-hydrophobic photocatalytic coating

    CN113683953A

  • Glass cleaning agent, self-cleaning glass, and preparation method thereof

    US20200024478A1

  • Method for preparing a self-cleaning transparent thermal insulation nanocoating

    US20230374229A1

Cited By

  • Hydrophobic and oleophobic modified epoxy resin as well as preparation method and application thereof