Cyano modified high-molecular polymer as well as synthesis method and application thereof
By performing multiple precipitation and high-temperature high-voltage electrocatalysis under low temperature conditions, the purity and dielectric properties of cyanograft modified polymers are improved, and the high dielectric loss and electrochemical stability in the prior art are solved. The problem of low performance is suitable for the manufacturing of high-performance electrochemical membranes.
Patent Information
- Application Number
- CN202411191753.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
In the synthesis method of cyanograft modified polymer, the dielectric loss is high, the electrochemical stability is low, and the by-products are many, resulting in insufficient water resistance and stability of the product, making it difficult to meet high-performance protons. Exchange membranes and lithium-ion battery separators are required.
The hydroxyl-containing polymer is mixed with acrylonitrile and strong polar solvent under constant low temperature conditions, and the initiator and strong alkaline catalyst are introduced, and multiple precipitation and purification are carried out through high-temperature and high-voltage electrocatalysis to form high purity. , cyano-modified polymer with low dielectric loss.
It improves the efficiency and uniformity of cyanograft reaction, has a large dielectric constant, low dielectric loss and high electrochemical stability, and is suitable for the manufacturing of high-performance electrochemical separators, reducing the cost of use.
Smart Images

Figure BDA0005015299390000051 
Figure BDA0005015299390000061 
Figure BDA0005015299390000081
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of new materials, and specifically relates to a cyano-modified high molecular polymer and a synthesis method and application thereof. Background Art
[0002] Hydroxyl-containing polymers are a class of widely used polymer materials, such as hydroxy acrylates, polyurethanes, acrylates, etc., which have good film-forming processability. However, due to the hygroscopicity of hydroxyl groups, the water resistance and stability of the film after formation are poor, which affects its application in electrical and electronic fields.
[0003] In the field of chemistry and chemical engineering, the Michael addition method is usually used to graft cyanide groups on the hydroxyl groups of high molecular polymers, introduce hydrophobic, negatively charged, highly polar cyanide functional groups, and obtain cyanide-grafted modified polymers, which retain the good film-forming properties of the raw polymer while enhancing its water resistance and stability.
[0004] The dielectric and electrochemical properties of polymers are closely related to their functional groups. The size of the dielectric constant depends on the polarization of the polar molecules. The stronger the polarity of the molecule and the greater the degree of polarization, the higher the dielectric constant. The cyano group is a strongly polar group with negative charge. The side chain cyano group is conducive to the orientation polarization to produce a large dipole moment. With the increase of the cyano grafting degree, the polymer has the characteristics of high polarization density and large dipole moment, and thus has a higher dielectric constant. Dielectric loss refers to the phenomenon that the dielectric itself heats up due to the consumption of part of the electrical energy in the alternating electric field. That is, under the action of the external alternating electric field, the material generates a conductive current, consumes part of the electrical energy, and converts it into heat energy. It is one of the important indicators of the performance of insulating materials. One of the factors affecting the dielectric loss of polymers is the dipole loss caused by impurities, by-products, additives or fillers in the polymer material. Therefore, the higher the purity of the polymer and the lower the by-products, the smaller its dielectric loss. The side chain cyano group exhibits good ionic conductivity, electrochemical stability and low interfacial resistance in the electrochemical process. Therefore, polymers rich in side chain cyano functional groups are the preferred materials for making various electrochemical membranes.
[0005] At present, there are many synthetic methods for cyano-grafting modification of side chain hydroxyl groups at home and abroad, and the resulting products have certain improvements in dielectric properties, electrochemical properties, water resistance, etc.
[0006] In patent CN1528799A, polyvinyl alcohol is used as raw material, and acrylonitrile is directly reacted with it under alkali catalysis to prepare cyanoethyl ether-β-polyvinyl alcohol, and the product has high dielectric constant and good film-forming property. However, since this synthesis method is carried out in an aqueous heterogeneous liquid system, acrylonitrile and grafted side chain cyano groups will be hydrolyzed under strong alkali and heating conditions, and the substitution degree and uniformity of the obtained product are extremely limited, and there are more by-products and the yield is low. The dielectric loss of the product is large and the electrochemical stability is low. The materials for high-performance proton exchange membranes and lithium ion battery separators are still unresolved key scientific and technological issues in this field. Summary of the invention
[0007] In order to solve the problems existing in the above-mentioned prior art, the present invention provides a cyano-modified high molecular polymer and a synthesis method and application thereof, the purpose of which is to use a hydroxyl-containing high molecular polymer as a raw material, and to perform cyano grafting modification on it under suitable reaction conditions and reaction systems, and to make the modified product have high purity and substitution degree, less impurities, large viscosity value and dielectric constant, low dielectric loss, high electrochemical stability, and high ionic conductivity. At the same time, the high bonding strength characteristics of the raw material are retained, and it can be used as a single component as a basic material to reduce the use cost, and the film thickness of the finished product is small, the mechanical properties and dielectric properties of the film are good, and the stability is strong.
[0008] In order to achieve the above object, the specific scheme of the present invention is as follows:
[0009] A method for synthesizing a cyano-modified high molecular polymer comprises the following steps:
[0010] Step 1, fully mixing a hydroxyl-containing polymer solution with a strong polar solvent;
[0011] Step 2, adding acrylonitrile to a mixture of a hydroxyl-containing high molecular polymer solution and a strong polar solvent, and mixing them thoroughly to form a reaction system;
[0012] Step 3, under constant low temperature conditions, drop an initiator into the reaction system and stir thoroughly; continue to drop a strong alkaline catalyst into the reaction system under the same constant low temperature conditions and keep stirring thoroughly;
[0013] Step 4, adding deionized water or ethanol to precipitate the polymer in the reaction system to form a flocculent precipitate 1; dissolving the flocculent precipitate 1 and then adding deionized water or ethanol again for precipitation, repeating 3 to 5 times to obtain a flocculent precipitate 2; drying the purified flocculent precipitate 2 and then fully dissolving it, and then subjecting it to high temperature and high pressure electrocatalysis to obtain a crude product solution, and then adding deionized water or ethanol to the crude product solution to precipitate to obtain a flocculent precipitate 3, and then fully dissolving the flocculent precipitate 3 and then adding deionized water or ethanol again for precipitation, and continuing to repeat 3 to 5 times to precipitate to obtain a purified flocculent precipitate;
[0014] Step 5, drying and crushing the purified flocculent precipitate to obtain cyano-modified polymer powder.
[0015] Furthermore, the degree of polymerization of the hydroxyl-containing polymer in step 1 is between 500 and 10,000, the molar percentage of the hydroxyl substitution degree is between 20% and 99%, the mass percentage concentration of the hydroxyl-containing polymer solution is between 5% and 50%; the mass ratio of the hydroxyl-containing polymer solution to the strong polar solvent is 1g:2-3g;
[0016] The hydroxyl-containing polymer includes but is not limited to hydroxy acrylate, polyurethane, and acrylate;
[0017] The highly polar solvent includes, but is not limited to, NN-dimethylformamide, N-methylpyrrolidone, and dimethyl sulfoxide.
[0018] Furthermore, the mass of the acrylonitrile in step 2 is 0.4 to 5 times the mass of the hydroxyl-containing high molecular polymer.
[0019] Furthermore, the initiator in step 3 accounts for 5% to 10% of the mass of the hydroxyl-containing high molecular polymer; the time for adding the initiator is controlled at 30 to 50 minutes, the constant low temperature reaction temperature is -20°C to 0°C, and the reaction time is 1 to 2 hours;
[0020] The strong alkaline catalyst accounts for 5% to 10% of the mass of the hydroxyl-containing high molecular polymer, and the mass percentage concentration of the strong alkaline catalyst is 20% to 40%; the time for dripping the strong alkaline catalyst is controlled at 30 to 50 minutes;
[0021] The initiator includes but is not limited to dimethyl azobisisobutyrate and 2,2'-azobisisobutyronitrile;
[0022] The strong alkaline catalyst includes but is not limited to sodium hydroxide solution and tetrabutylammonium fluoride solution.
[0023] Furthermore, the temperature of the high temperature and high pressure electrocatalysis in step 4 is 90° C. to 120° C., the pressure is 0.7 MPa to 1.5 MPa, and the high temperature and high pressure electrocatalysis reaction time is 0.5 to 1 h;
[0024] The electrocatalytic medium includes but is not limited to platinum and platinum-palladium catalysts, and the current is 1 to 10A.
[0025] A cyano-modified high molecular polymer powder prepared by the synthesis method.
[0026] The cyano-modified high molecular polymer powder is used in manufacturing high-performance electrochemical diaphragms.
[0027] The electrochemical diaphragm manufactured by using the cyano-modified high molecular polymer powder includes but is not limited to a high-performance proton exchange membrane and a high-rate lithium-ion battery diaphragm.
[0028] A product using the electrochemical diaphragm, including but not limited to lithium-ion batteries and hydrogen fuel cells.
[0029] Advantages of the present invention
[0030] 1. The synthesis method of the present invention uses hydroxyl-containing polymer and acrylonitrile as raw materials, and dissolves the raw materials in the early stage of the synthesis reaction, mixes the hydroxyl-containing polymer solution with a co-solvent of acrylonitrile and a reaction processing solvent, dissolves the hydroxyl-containing polymer and mixes it with a strong polar solvent, and sequentially initiates with an initiator and catalyzes with a high-concentration strong alkaline catalyst at a constant low temperature, and then performs secondary modification by a high-temperature and high-pressure electrocatalytic method to synthesize a cyano-modified polymer, which not only improves the reaction efficiency of cyano grafting, but also the reaction is always carried out in a liquid homogeneous system, so that the modification reaction is more sufficient and uniform, and the substitution degree and purity, dielectric properties, and electrochemical properties of the product are greatly improved. The modified product has high purity and substitution degree, few impurities, large viscosity value and dielectric constant, low dielectric loss, high electrochemical stability, and high ionic conductivity. At the same time, the characteristics of high bonding strength of the raw material are retained, and it can be used as a single component as a basic material, which reduces the cost of use, the film thickness of the finished product is small, the mechanical properties and dielectric properties of the film are good, and the stability is strong. It also expands the product application field and overcomes product defects caused by the shortcomings of traditional synthesis methods.
[0031] 2. The synthesis method of the present invention uses a two-phase or single-phase blend of a solution of a hydroxyl-containing polymer and acrylonitrile as a reaction system, dissolves the hydroxyl-containing polymer and mixes it with acrylonitrile as a reaction solvent, and sequentially initiates with a low-temperature high-concentration initiator, catalyzes with a low-temperature high-concentration strong base, and electrocatalyzes with a high temperature and high pressure, and efficiently and efficiently and efficiently grafts cyanide groups on the hydroxyl-containing polymer in a two-phase or single-phase liquid system to obtain a cyano-modified polymer containing negatively charged cyano groups and having strong polarity. The purity of the product prepared from the cyano-modified polymer powder can reach more than 99%, and the dielectric constant value of the membrane material manufactured from it exceeds 20, and has an ultra-low dielectric loss of less than 0.01%. It has become an upgraded product of traditional organic dielectric film-forming resins, and is particularly suitable for the manufacture of high-performance electrochemical diaphragms, such as high-performance proton exchange membranes and high-rate lithium-ion battery diaphragms.
[0032] 3. The cyano-modified high molecular polymer prepared by the present invention can greatly improve the microscopic interface ion transport kinetics of electrochemical devices due to its abundant strong polar cyano side chain groups. At the same time, due to the original step-by-step low-temperature initiation, catalysis and high-temperature and high-pressure electrocatalysis, the grafting degree of the product is greatly improved, and the by-products are extremely low. The obtained product has excellent film-forming and fiber-forming properties as well as good mechanical properties and temperature resistance, and is a high-quality raw material for electrochemical diaphragms. DETAILED DESCRIPTION
[0033] The present invention is further explained below in conjunction with specific implementation methods. It should be noted that this specific embodiment is not intended to limit the scope of rights of the present invention.
[0034] Embodiment 1
[0035] The first embodiment provides a cyano-modified high molecular polymer and a synthesis method and application thereof, wherein the synthesis method comprises the following steps:
[0036] Step 1, placing a four-necked flask equipped with a stirrer and a thermometer in a -20°C constant temperature water area, adding 4 g of a hydroxyl-containing high molecular polymer having a degree of polymerization of 1000 and a molar percentage of hydroxyl substitution of 40% as hydroxyl acrylate into the flask in sequence, dissolving the hydroxyl acrylate in an ethanol solution at a mass percentage concentration of 20%, then adding 12 ml of NN-dimethylformamide as a strong polar solvent and mixing well, stirring for 30 minutes until the liquid is completely transparent, to form a hydroxyl-containing high molecular polymer solution;
[0037] Since different hydroxyl-containing polymers have different solubilities in strong polar solvents, a good solvent for the hydroxyl-containing polymer is first used to prepare a polymer solution. The hydroxyl-containing polymer selected in this embodiment is hydroxy acrylate, and its dissolved mass percentage concentration is 20%. The strong polar solvent selected is dimethylformamide, which is used as a co-solvent and processing solvent for the hydroxy acrylate solution and acrylonitrile. Since the strong polar solvent has good miscibility with water and other organic solvents, it is a good processing solvent in the acrylonitrile reaction, which can accelerate the cyanide grafting speed, reduce the generation of side reactants, and improve the yield.
[0038] Step 2, add 20 ml of acrylonitrile and continue stirring to fully mix to form a reaction system;
[0039] Step 3, under a constant low temperature condition of -20°C, slowly drop 0.3 ml of an initiator, which is dimethyl azobisisobutyrate, into the bottle in the reaction system at a flow rate of 0.01 ml / min within 30 minutes, and keep stirring well; and under the same constant low temperature condition, continue to slowly drop 1.5 ml of a 20% mass percentage concentration of sodium hydroxide solution as a strong alkaline catalyst into the bottle in the reaction system at a flow rate of 0.05 ml / min within 30 minutes, and keep stirring well for 30 minutes;
[0040] In the conventional process, the amount of initiator used is usually less than 5% of the mass of the reactants, and the reaction must be carried out for a long time under heating conditions. The conventional method will cause more side reactions and acrylonitrile self-polymerization. However, the present embodiment first initiates the reaction with an initiator, and uses a large dose of initiator accounting for 5% to 10% of the mass of the hydroxy acrylate at a low temperature of -20°C to 0°C and shortens the reaction time, which can effectively avoid the side reactions and acrylonitrile self-polymerization caused by long-term heating.
[0041] In the traditional process, the amount of strong alkaline catalyst used is less than 5% of the mass of the reactants, and the mass percentage concentration of the strong alkaline catalyst solution is less than 20%, and it needs to be carried out for a long time under heating conditions. The traditional method will cause more side reactions, as well as acrylonitrile self-polymerization and hydrolysis reactions. In order to improve the grafting degree and yield, this embodiment uses a large dose of initiator accounting for 5% to 10% of the mass of hydroxy acrylate at a low temperature of -20°C to 0°C and a sodium hydroxide solution with a mass percentage concentration of 20% to 40% as a strong alkaline catalyst and shortens the reaction time, which can effectively avoid side reactions caused by long-term heating, acrylonitrile self-polymerization and hydrolysis reactions.
[0042] Step 4, adding deionized water or ethanol to precipitate the polymer in the reaction system to form a flocculent precipitate 1; after dissolving the flocculent precipitate, adding deionized water or ethanol again for precipitation, repeating 3 to 5 times to obtain a flocculent precipitate 2; drying the purified flocculent precipitate 2 and fully dissolving it, and subjecting the temperature to 90° C. and the pressure to 0.9 MPa, using an electrocatalytic medium including but not limited to platinum and platinum-palladium catalysts for high-temperature and high-pressure electrocatalysis, controlling the current to 2A, to obtain a crude product solution, and then adding deionized water or ethanol to the crude product solution to precipitate to obtain a flocculent precipitate 3, and then fully dissolving the flocculent precipitate 3 and adding deionized water or ethanol again for precipitation, and continuing to repeat 3 to 5 times to precipitate to obtain a purified flocculent precipitate;
[0043] Step 5: Dry and crush the purified flocculent precipitate to obtain cyano-modified polymer powder. The powdered raw material that is easy to store and transport can be obtained by atomization drying.
[0044] A cyano-modified high molecular polymer powder prepared by the above synthesis method.
[0045] An application of the cyano-modified high molecular polymer powder in manufacturing high-performance electrochemical diaphragms.
[0046] The electrochemical diaphragm manufactured by using the cyano-modified high molecular polymer powder includes but is not limited to a high-performance proton exchange membrane and a high-rate lithium-ion battery diaphragm.
[0047] A product using the electrochemical diaphragm, including but not limited to lithium-ion batteries and hydrogen fuel cells.
[0048] The cyano-modified polymer powder obtained in Example 1 is dissolved in dimethylformamide, dimethyl sulfoxide or acetone at a mass percentage of 10-20%, and a nanoporous non-woven fiber membrane with a certain thickness and a wire diameter of 50-1000 nanometers is manufactured using electrospinning equipment and technology, and is cut into a film product of a certain shape and size. The film product can replace the traditional PE and PP commercial diaphragms and be used to manufacture various high-performance lithium-ion batteries. The purity of the product made from the cyano-modified polymer powder can reach more than 99%, and the dielectric constant value of the membrane material manufactured from it exceeds 20, and has an ultra-low dielectric loss of less than 0.01%.
[0049] Specifically, the cyano-modified polymer powder obtained in Example 1 was dissolved in dimethylformamide at a mass percentage of 20%, and the film product properties obtained by using electrospinning equipment and process were as follows:
[0050]
[0051]
[0052] The performance of a lithium-ion battery with a capacity of 1 Ah manufactured using NCM811 as the positive electrode material and graphite as the negative electrode material using the thin film product of Example 1 is as follows:
[0053] Under 5C rate conditions, the capacity retention rate is 90% after 300 cycles of charge and discharge;
[0054] Under 10C rate conditions, the capacity retention rate is 87% after 300 cycles of charge and discharge.
[0055] Embodiment 2
[0056] The second embodiment provides a cyano-modified high molecular polymer and a synthesis method and application thereof, wherein the synthesis method comprises the following steps:
[0057] Step 1, placing a four-necked flask equipped with a stirrer and a thermometer in a 2°C constant temperature water area, adding 4 g of a hydroxyl-containing polymer polyvinyl alcohol having a degree of polymerization of 10,000 and a molar percentage of hydroxyl substitution of 99% into the flask, dissolving the polyvinyl alcohol in water at a mass percentage concentration of 20%, adding 12 g of dimethyl sulfoxide as a strong polar solvent and mixing well, stirring for 30 minutes until the liquid is completely transparent, to form a hydroxyl-containing polymer solution;
[0058] The highly polar solvent selected is dimethyl sulfoxide, which is used as a co-solvent and processing solvent for the polyvinyl alcohol solution and acrylonitrile. Since the highly polar solvent has good miscibility with water and other organic solvents, it is a good processing solvent in the acrylonitrile reaction, which can accelerate the cyanide grafting speed, reduce the generation of side reactants, and improve the yield.
[0059] Step 2, add 20 ml of acrylonitrile and continue stirring to fully mix to form a reaction system;
[0060] Step 3, under a constant low temperature condition of 2° C., slowly drop 0.4 ml of an initiator, which is dimethyl azobisisobutyrate, into the bottle in the reaction system at a flow rate of 0.008 ml / min within 50 min, and keep stirring sufficiently; and under the same constant low temperature condition, continue to slowly drop 1.5 ml of a strong alkaline catalyst, which is a sodium hydroxide solution, with a mass percentage concentration of 20%, into the bottle in the reaction system at a flow rate of 0.05 ml / min within 30 min, and keep stirring sufficiently for 30 min;
[0061] In this embodiment, a large dose of initiator accounting for 10% of the mass of polyvinyl alcohol is used to initiate the reaction at a low temperature of 2° C., and the reaction time is shortened, which can effectively avoid the side reactions and acrylonitrile self-polymerization caused by long-term heating.
[0062] In order to improve the grafting degree and yield, after the initiator initiates the reaction, a large dose of high-concentration sodium hydroxide solution with a mass percentage concentration of 20% is used as a strong alkaline catalyst at a low temperature of 2°C and the reaction time is shortened, which can effectively avoid side reactions, acrylonitrile self-polymerization and hydrolysis reactions caused by long-term heating.
[0063] Step 4, adding deionized water or ethanol to precipitate the polymer in the reaction system to form a flocculent precipitate 1; after dissolving the flocculent precipitate, adding deionized water or ethanol again for precipitation, repeating 3 to 5 times to obtain a flocculent precipitate 2; drying the purified flocculent precipitate 2 and fully dissolving it, and subjecting the purified flocculent precipitate 2 to high temperature and high pressure electrocatalysis at a temperature of 90° C. and a pressure of 0.9 MPa, using an electrocatalytic medium including but not limited to platinum and platinum-palladium catalysts, and controlling the current to 10 A to obtain a crude product solution, and then adding deionized water or ethanol to the crude product solution to precipitate to obtain a flocculent precipitate 3, and then fully dissolving the flocculent precipitate 3 and adding deionized water or ethanol again for precipitation, and continuing to repeat 3 to 5 times to precipitate to obtain a purified flocculent precipitate;
[0064] Step 5: Dry and crush the purified flocculent precipitate to obtain cyano-modified polymer powder. The powdered raw material that is easy to store and transport can be obtained by atomization drying.
[0065] Specifically, the cyano-modified polymer powder obtained in Example 2 was dissolved in dimethylformamide at a mass percentage of 10%, and the film product properties obtained by using ultrasonic spraying equipment and process were as follows:
[0066] index data unit Liquid absorption rate 290 % Tensile Strength 67 MPa Porosity 52 % Air resistance 119 s / 100ml Dielectric constant 21.2 N / A Dielectric loss 0.005 % Puncture strength 362 <![CDATA[g·μm -1 ]]> Average pore size 400 nm thickness 0.02 mm
[0067] The performance of a lithium-ion battery with a capacity of 1Ah manufactured using NCM622 as the positive electrode material and graphite as the negative electrode material using the thin film product of Example 2 is as follows:
[0068] Under 5C rate conditions, the capacity retention rate is 86% after 500 cycles of charge and discharge;
[0069] Under 10C rate conditions, the capacity retention rate is 82% after 500 cycles of charge and discharge.
[0070] Embodiment 3
[0071] The third embodiment provides a cyano-modified high molecular polymer and a synthesis method and application thereof, wherein the synthesis method comprises the following steps:
[0072] Step 1, placing a four-necked flask equipped with a stirrer and a thermometer in a constant temperature water area of 0°C, adding 4g of a hydroxyl-containing high molecular polymer with a degree of polymerization of 500 and a molar percentage of hydroxyl substitution of 20% as polyurethane into the flask, dissolving the polyurethane in a methylpyrrolidone solution at a mass percentage concentration of 20%, adding 8g of dimethylformamide and mixing well, stirring for 50min until the liquid is completely transparent, to form a hydroxyl-containing high molecular polymer solution;
[0073] The highly polar solvent selected is dimethylformamide, which is used as a co-solvent and processing solvent for the polyurethane solution and acrylonitrile. Since the highly polar solvent has good miscibility with water and other organic solvents, it is a good processing solvent in the acrylonitrile reaction, which can accelerate the cyanide grafting speed, reduce the generation of side reactants, and improve the yield.
[0074] Step 2, add 20 ml of acrylonitrile and continue stirring to fully mix to form a reaction system;
[0075] Step 3, under a constant low temperature condition of 0°C, slowly drop 0.3 ml of an initiator, which is dimethyl azobisisobutyrate, into the bottle in the reaction system at a flow rate of 0.01 ml / min within 30 minutes, and keep stirring sufficiently; and under the same constant low temperature condition, continue to slowly drop 1.5 ml of a 15% mass percentage concentration of tetrabutylammonium fluoride solution as a strong alkaline catalyst into the bottle in the reaction system at a flow rate of 0.05 ml / min within 30 minutes, and keep stirring sufficiently for 30 minutes;
[0076] This embodiment firstly uses a large dose of initiator accounting for 7.5% of the mass of the polyurethane to initiate the reaction at a low temperature of 0°C and shortens the reaction time, which can effectively avoid the side reactions and acrylonitrile self-polymerization caused by long-term heating.
[0077] In order to improve the grafting degree and yield, after the initiator initiates the reaction, a large dose of high-concentration tetrabutylammonium fluoride solution with a mass percentage concentration of 15% is used as a strong alkaline catalyst at a low temperature of 0°C and the reaction time is shortened, which can effectively avoid side reactions caused by long-term heating, acrylonitrile self-polymerization and hydrolysis reactions.
[0078] Step 4, adding deionized water or ethanol to precipitate the polymer in the reaction system to form a flocculent precipitate 1; after dissolving the flocculent precipitate, adding deionized water or ethanol again for precipitation, repeating 3 to 5 times to obtain a flocculent precipitate 2; drying the purified flocculent precipitate 2 and fully dissolving it, and subjecting the temperature to 90° C. and the pressure to 0.9 MPa, using an electrocatalytic medium including but not limited to platinum and platinum-palladium catalysts for high temperature and high pressure electrocatalysis, controlling the current to 5A, to obtain a crude product solution, and then adding deionized water or ethanol to the crude product solution to precipitate to obtain a flocculent precipitate 3, and then fully dissolving the flocculent precipitate 3 and adding deionized water or ethanol again for precipitation, and continuing to repeat 3 to 5 times to precipitate to obtain a purified flocculent precipitate;
[0079] Step 5: Dry and crush the purified flocculent precipitate to obtain cyano-modified polymer powder. The powdered raw material that is easy to store and transport can be obtained by atomization drying.
[0080] Specifically, the cyano-modified polymer powder obtained in Example 3 was dissolved in dimethylformamide at a mass percentage of 15%, and the film product properties obtained by using the slit coating equipment and process were as follows:
[0081]
[0082]
[0083] The performance of a 10W hydrogen fuel cell manufactured using the film product of Example 3 is as follows:
[0084] The stack temperature is less than 50°C, the mass power density is 750W / Kg, the volume power density is 5.6KW / L, and the life is 30,000 hours.
Claims
1. A method for synthesizing a cyano-modified high molecular polymer, characterized in that: The steps include: Step 1, fully mixing a hydroxyl-containing polymer solution with a strong polar solvent; Step 2, adding acrylonitrile to a mixture of a hydroxyl-containing high molecular polymer solution and a strong polar solvent, and mixing them thoroughly to form a reaction system; Step 3, under constant low temperature conditions, adding an initiator to the reaction system and stirring thoroughly; continuing under the same constant low temperature conditions, adding a strong alkaline catalyst dropwise to the reaction system and maintaining sufficient stirring; Step 4, adding deionized water or ethanol to precipitate the polymer in the reaction system to form a flocculent precipitate 1; dissolving the flocculent precipitate 1 and then adding deionized water or ethanol again for precipitation, repeating 3 to 5 times to obtain a flocculent precipitate 2; drying the purified flocculent precipitate 2 and fully dissolving it, and then subjecting it to high temperature and high pressure electrocatalysis to obtain a crude product solution, and then adding deionized water or ethanol to the crude product solution to precipitate to obtain a flocculent precipitate 3, and then fully dissolving the flocculent precipitate 3 and then adding deionized water or ethanol again for precipitation, and continuing to repeat 3 to 5 times to precipitate to obtain a purified flocculent precipitate; Step 5, drying and crushing the purified flocculent precipitate to obtain cyano-modified polymer powder.
2. The synthesis method according to claim 1, characterized in that Step 1: the polymerization degree of the hydroxyl-containing polymer is between 500 and 10,000, the molar percentage of the hydroxyl substitution degree is between 20% and 99%, the mass percentage concentration of the hydroxyl-containing polymer solution is between 5% and 50%, and the mass ratio of the hydroxyl-containing polymer solution to the strong polar solvent is 1g:2-3g; The hydroxyl-containing polymer includes but is not limited to hydroxy acrylate, polyurethane, and acrylate; The highly polar solvent includes, but is not limited to, N,N-dimethylformamide, N-methylpyrrolidone, and dimethyl sulfoxide.
3. The synthesis method according to claim 1, characterized in that The mass of the acrylonitrile in step 2 is 0.4 to 5 times the mass of the hydroxyl-containing high molecular polymer.
4. The synthesis method according to claim 1, characterized in that The initiator in step 3 accounts for 5% to 10% of the mass of the hydroxyl-containing high molecular polymer; the time for adding the initiator is controlled at 30 to 50 minutes, the constant low temperature reaction temperature is -20°C to 0°C, and the reaction time is 1 to 2 hours; The strong alkaline catalyst accounts for 5% to 10% of the mass of the hydroxyl-containing high molecular polymer, and the mass percentage concentration of the strong alkaline catalyst is 20% to 40%; the time for dripping the strong alkaline catalyst is controlled at 30 to 50 minutes; The initiator includes but is not limited to dimethyl azobisisobutyrate and 2,2'-azobisisobutyronitrile; The strong alkaline catalyst includes but is not limited to sodium hydroxide solution and tetrabutylammonium fluoride solution.
5. The synthesis method according to claim 1, characterized in that The temperature of the high temperature and high pressure electrocatalysis in step 4 is 90° C. to 120° C., the pressure is 0.7 MPa to 1.5 MPa, and the high temperature and high pressure electrocatalysis reaction time is 0.5 to 1 h; The electrocatalytic medium includes but is not limited to platinum and platinum-palladium catalysts, and the current is 1 to 10A.
6. A cyano-modified high molecular polymer powder prepared by the synthesis method according to any one of claims 1 to 5.
7. Use of the cyano-modified polymer powder according to claim 6 in the manufacture of high-performance electrochemical diaphragms.
8. An electrochemical membrane manufactured using the cyano-modified high molecular polymer powder according to claim 6, wherein the electrochemical membrane includes but is not limited to a high-performance proton exchange membrane and a high-rate lithium-ion battery membrane.
9. A product using the electrochemical membrane of claim 8, the product including but not limited to lithium-ion batteries and hydrogen fuel cells.
Citation Information
Patent Citations
Modified synthesis method for high-viscosity film forming resin with dielectric property
CN102344511A
Preparation method and application of modified polyvinyl alcohol resin
CN102942645A
Electrostatic spinning modified lithium ion battery diaphragm as well as preparation method and application thereof
CN118299758A
Electroluminous phenothiazine polymer material and its prepn process
CN1740266A