Method for preparing phenolic resin from phenol rectification residues

The m-propol resin is generated by reacting inter-poroisopropol with formaldehyde, and the unreacted phenolic substances are extracted through distillation and dehydration steps, which solves the problem of utilization of phenolic distillation residues, and achieves high-quality phenolic resins and high-purity phenols The extraction of substances improves the simplicity and economic benefits of the process.

CN118930774APending Publication Date: 2024-11-12YANCHENG INST OF TECH
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411172831.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The prior art cannot effectively utilize phenolic distillation residues, especially because phenolic substances with complex composition and similar properties cannot be distilled and separated, resulting in failure to fully utilize them, limiting the synthesis and application of phenolic resins.

Method used

Low molecular weight m-propol resin is generated by reacting m-propol and formaldehyde, and unreacted phenol substances such as isopropol and p-propol are extracted through distillation and dehydration steps. , realize the synthesis of phenolic resin and the extraction of phenolic substances.

Benefits of technology

The preparation of m-propfol novolac resin with narrow molecular weight distribution, good corrosion resistance and light color was achieved. At the same time, high-purity paraisopropfol and other materials were extracted, which improved the simplicity and economic benefits of the process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005009815700000051
    Figure BDA0005009815700000051
  • Figure BDA0005009815700000061
    Figure BDA0005009815700000061
  • Figure BDA0005009815700000062
    Figure BDA0005009815700000062
Patent Text Reader

Abstract

The invention relates to the technical field of organic synthesis, in particular to a method for preparing phenolic resin from phenol rectification residues. The method comprises the following specific steps: S1, carrying out rectification separation on the phenol rectification residues to obtain m-p-isopropyl phenol / m-p-propyl phenol / 2, 3-methyl ethyl phenol raw materials; s2, adding aldehydes into the raw materials obtained in S1 for reaction, and introducing steam for steam distillation to remove free phenol; heating, decompressing and dehydrating the free phenol-removed material to obtain m-propyl phenol-formaldehyde resin; and S3, preparing thermosetting resin or thermoplastic resin by using p-isopropyl phenol / p-propyl phenol / 2, 3-methyl ethyl phenol obtained by layering a dehydrated water layer after synthesis of the phenolic resin in S2. According to the invention, the m-propyl phenolic resin with high content and high price is directly produced by utilizing the difference between the reactivity of m-p-isopropyl phenol / m-p-propyl phenol and formaldehyde, and can be used as a film material for photoresist; and unreacted phenols are distilled out, and high-quality products are produced through rectification, so that the process is simple, the operation is convenient, and the added value is high.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of organic synthesis, and in particular to a method for preparing phenolic resin by utilizing phenol distillation residues. Background Art

[0002] At present, the price of xylenol distillation residue and crude phenol distillation residue is only 2000-3000 yuan / ton. The price is low and can only be used as fuel oil. Many phenolic substances such as 3,4-xylenol, 2,3,6-trimethylol, m-p-isopropylphenol, m-p-propylphenol, 3-methyl-5-ethylphenol, 2,3,5-trimethylol, 2,3-methylethylphenol, 3,4-methylethylphenol have not been utilized; since m-isopropylphenol / m-propylphenol, p-isopropylphenol / p-propylphenol, 2,3-methylethylphenol have similar boiling points, distillation separation is impossible; due to the complex composition and similar properties, alkylation cannot separate m-isopropylphenol and m-propylphenol, p-isopropylphenol / p-propylphenol, so there is currently no good treatment method.

[0003] The main properties of m-p-isopropylphenol (which may contain some m-p-propylphenol) are relatively close to those of m-p-cresol and m-p-ethylphenol. Therefore, most of the application fields of m-p-cresol and m-p-ethylphenol can be replaced by m-p-isopropylphenol, and it is widely used in the production of insulating wire enameling paint, flame retardant plasticizers, photoresists, etc.; m-p-isopropylphenol can also be used to separate and produce pure m-isopropylphenol and p-isopropylphenol and its derivatives, and then p-isopropylphenol can be converted into m-p-isopropylphenol with a transposition catalyst; p-propylphenol can also be converted into m-isopropylphenol in the presence of a high-temperature transposition catalyst, and a small amount can be converted into m-propylphenol, which further improves the price and application value of m-p-isopropylphenol.

[0004] In the extraction of crude phenol from coal tar or gasification of crude phenol, m-p-isopropylphenol / propylphenol mainly exists in the residue after distillation of xylenol. This mixture can be extracted by distillation. The boiling point is 228-231°C. It is mainly composed of m-p-isopropylphenol, m-p-propylphenol, 2,3-methylethylphenol, and also contains 3,4-xylenol, 3-ethyl-5-methylphenol, 2,3,5-trimethylphenol, etc., while 2,4,5-trimethylphenol and 2,3,6-trimethylphenol are rare. Since m-isopropylphenol and m-propylphenol can react with aldehydes to synthesize cross-linked and stereotyped resins, p-isopropylphenol, propylphenol, 2,3-methylethylphenol, 3,4-xylenol, 3-ethyl-5-methylphenol, 2,3,5-trimethylphenol, etc. -5-Cresol, 2,3,5-trimethylphenol, etc. can also react with aldehydes to obtain linear phenolic resins. In the synthesis of phenolic resins, it is necessary to control the content of 2,4,5-trimethylphenol, 2,3,6-trimethylphenol, 2,4-methylethylphenol, etc. Analysis has confirmed that the content of 2,4,5-trimethylphenol and 2,3,6-trimethylphenol in the crude phenol extracted from the tar or water obtained by gasification of most types of coal is below 0.01%, which is less than 0.5% of that of m-isopropylphenol / m-isopropylphenol and 2,3-methylethylphenol. By utilizing the differences in boiling point and relative volatility, distillation can obtain m-isopropylphenol / m-isopropylphenol raw materials that meet the needs of phenolic resin synthesis.

[0005] Therefore, in order to broaden the scope of utilization of crude phenol distillation residue, it is of great significance to develop a new method for preparing phenolic resin using phenol distillation residue. Summary of the invention

[0006] Purpose of the invention: The technical problem to be solved by the present invention is to provide a method for utilizing the huge difference in the reaction activity of m-p-isopropylphenol / m-p-propylphenol / 2,3-methylethylphenol with formaldehyde to react m-p-isopropylphenol / m-p-propylphenol / 2,3-methylethylphenol with formaldehyde to generate a low molecular weight m-propanol-aldehyde resin, and then distill off the free unreacted p-isopropylphenol, p-propylphenol, 2,3-methylethylphenol, etc., and then slowly polymerize while heating and dehydrating, and dehydrating to 190-200°C and keeping warm to obtain a m-propanol-aldehyde photoresist with a narrow molecular weight distribution, good corrosion resistance and light color, thereby achieving the purpose of extracting p-isopropylphenol, p-propylphenol and 2,3-methylethylphenol while synthesizing the m-propanol-aldehyde resin. The reaction activity of 3-ethyl-5-methylphenol, meta-isopropylphenol / meta-propylphenol with formaldehyde is significantly higher than that of p-isopropylphenol / propylphenol, 2,3-methylethylphenol, 3,4-dimethylphenol, 2,3,5-trimethylphenol, etc. Therefore, when p-isopropylphenol / propylphenol reacts with formaldehyde, after the reaction of meta-isopropylphenol and meta-propylphenol is completed, there is still a lot of p-isopropylphenol / propylphenol in the system that has not reacted and exists in the form of free phenol; at this time, distillation and dehydration are performed to evaporate the unreacted p-isopropylphenol, p-propylphenol or a mixture thereof, and pure p-isopropylphenol or p-propylphenol can be further extracted. The present invention can obtain materials such as p-isopropylphenol while synthesizing phenolic resin.

[0007] In order to solve the above technical problems, the present invention discloses a method for preparing phenolic resin using phenol distillation residue, and the specific steps are as follows:

[0008] S1. distilling and separating the phenol distillation residue to obtain m-isopropylphenol / m-propylphenol / 2,3-methylethylphenol raw materials;

[0009] S2. Add aldehydes to the meta-isopropylphenol / meta-propylphenol / 2,3-methylethylphenol raw materials obtained in S1, and then steam distill to remove free phenol; the material from which free phenol is removed is heated and decompressed to obtain meta-propylphenol-formaldehyde resin;

[0010] S3. preparing a thermosetting resin or a thermoplastic resin by using the p-isopropylphenol / p-propylphenol / 2,3-methylethylphenol obtained by dehydrating the water layer in the phenolic resin synthesis in S2;

[0011] The phenolic distillation residue includes one of a xylenol distillation residue and a crude phenol distillation residue. Preferably, the phenolic distillation residue is a xylenol distillation residue;

[0012] More preferably, the distillation residue of xylenol refers to the fraction with a distillation range of 226-235°C, which is composed of 0-2wt% of p-ethylphenol, 0-3wt% of m-ethylphenol, 0-5wt% of 3,5-xylenol, 0-5wt% of 2,4,6-trimethylphenol, 0-15wt% of 3,4-xylenol, 0-5wt% of 2,3,6-trimethylphenol, 0-5wt% of 2,4- / 2,5-methylethylphenol, 0-10wt% of 2,3-methylethylphenol, 10-30wt% of 3-ethyl-5-methylphenol, 0-20wt% of p-isopropylphenol, 0-25wt% of m-isopropylphenol, 0-10wt% of p-propylphenol, 0-15wt% of m-propylphenol, 5-30wt% of 2,3,5-trimethylphenol and 0-1wt% of 2,4,5-trimethylphenol.

[0013] The specific steps of S1 are as follows: adding phenol distillation residue to a stirred reactor, starting stirring, heating to 110-150° C., adding concentrated sulfuric acid dropwise for treatment, transferring the material to a high-efficiency distillation tower kettle for distillation, and obtaining m-isopropylphenol / m-propylphenol / 2,3-methylethylphenol raw materials at the top of the tower after reflux dehydration;

[0014] Preferably, in S1, the amount of concentrated sulfuric acid added is 0.2-1wt% of the phenol distillation residue; the distillation conditions are 200-350 plate numbers, -0.05-0.1Mpa vacuum, and a reflux ratio of (15-30):1.

[0015] More preferably, the meta-isopropylphenol / meta-propylphenol / 2,3-methylethylphenol raw material refers to a fraction with a distillation range of 227-231°C, consisting of 0-1wt% of 3,5-xylenol, 0-5wt% of 3,4-xylenol, 0-0.3wt% of 2,3,6-tricresol, 0-0.3wt% of 2,4- / 2,5-methylethylphenol, 1-15wt% of 2,3-methylethylphenol, 1-5wt% of 3-ethyl-5-methylphenol, 10-40wt% of p-isopropylphenol, 15-60wt% of meta-isopropylphenol, 1-30wt% of p-propylphenol, 1-50wt% of meta-propylphenol, 0-5wt% of 2,3,5-tricresol, and 0-0.2wt% of 2,4,5-tricresol.

[0016] The specific steps of S2 are as follows: adding the meta-isopropylphenol / meta-propylphenol / 2,3-methylethylphenol raw materials and catalyst separated in S1 into a reactor, starting stirring, heating to 80-100° C., adding aldehydes for reaction, adding for 4-6 hours, keeping warm for 1-2 hours after adding, sampling and analyzing, liquid phase or gel chromatography analysis shows that the meta-isopropylphenol / meta-propylphenol content is less than 0.5% and is qualified, steam is introduced for water vapor distillation to remove free phenol, the evaporated water layer is allowed to stand to separate the oil layer, the water layer is extracted twice with a water-insoluble solvent, and then the organic layer is combined, the organic layer is distilled to obtain a solvent, and further distilled to obtain one or more mixtures of p-isopropylphenol, p-propylphenol and 2,3-methylethylphenol;

[0017] After the free phenol is evaporated, the phenolic resin is heated and decompressed to dehydrate until the temperature reaches 190-200°C for 2-3 hours, and then kept warm for 1-2 hours. The vacuum is broken with nitrogen, and the material is discharged while hot to a stainless steel material tray under nitrogen protection to obtain a propanol-formaldehyde resin product, which is used as a film material for photoresist or a phenolic resin.

[0018] Preferably, in S2, the catalyst comprises a mixture of one or more of oxalic acid, formic acid, phosphoric acid, benzoic acid and benzenesulfonic acid; the amount of the catalyst is 0.1-5wt% of the raw material of m-isopropylphenol / m-isopropylphenol / 2,3-methylethylphenol; the aldehyde comprises one or more of paraformaldehyde, formaldehyde and acetaldehyde; the amount of the aldehyde is 0.5-0.9 of the molar amount of phenol; the non-water-soluble solvent comprises one of benzene, chlorinated hydrocarbons, chlorinated benzenes, ethers, ketones and esters;

[0019] More preferably, in S2, the amount of the catalyst is 0.5-1.5% of the m-isopropylphenol / m-propylphenol / 2,3-methylethylphenol raw material, the catalyst is oxalic acid or a mixture of oxalic acid / formic acid, the mass ratio of the mixture of oxalic acid and formic acid is (1-5):1; the aldehyde is formaldehyde; and the non-water-soluble solvent is toluene.

[0020] More preferably, in the further distillation in S2 to obtain a mixture of one or more of p-isopropylphenol, p-propylphenol and 2,3-methylethylphenol, the content of p-isopropylphenol / p-propylphenol / 2,3-methylethylphenol mixture is ≥ 98%, wherein p-isopropylphenol is 0-100%, p-propylphenol is 0-100% and 2,3-methylethylphenol is 0-80%.

[0021] Among them, in S3, the specific steps of preparing the thermosetting resin are: start stirring, add the p-isopropylphenol / p-propylphenol / 2,3-methylethylphenol obtained by dehydrating the water layer after the phenolic resin synthesis in S2 into the reactor; add the m-isopropylphenol / m-p-propylphenol / 2,3-methylethylphenol obtained in S1 in batches, and the first addition uses 60-100% of the total amount; then add alkali, turn off the steam when the temperature is about 50-75°C, slowly increase the temperature to 80-95°C, turn on the cooling water, add or drip aldehydes in batches for reaction, the dripping time is 2-4 hours, add the remaining m-isopropylphenol / m-p-propylphenol / 2,3-methylethylphenol raw materials after dripping, and keep the temperature for reaction for 1-3 hours;

[0022] After the reaction is completed, add a medium or weak acid to neutralize to neutrality, maintain neutrality for more than 10 minutes, and re-test for neutrality to be qualified. Turn on the vacuum pump and start dehydration. When the dehydration speed slows down or the temperature drops to about 70-75°C, turn on steam heating. During dehydration, the steam switch should be continuously adjusted according to the speed of water output to complete the dehydration at a lower temperature as much as possible. In the later stage, steam can be continuously passed to control the final temperature of the liquid at 80-90°C until the water level is reduced to 80% of the mass of the phenolic material. Samples are taken for analysis of water content and viscosity. When the water content is 2-3%, stop vacuuming, add an appropriate amount of ethylene glycol to condition the viscosity, and adjust the viscosity to a specified value of 15-20 Pa.s. After the viscosity reaches the requirement, the temperature is lowered to 50°C to discharge the material to obtain the thermosetting resin.

[0023] Preferably, in S3, in the process of preparing the thermosetting resin, the base includes one or more of alkali metal hydroxides, alkaline earth metal hydroxides, carbonates, bicarbonates, ammonia water, alcoholamines and hydroxylamines; the amount of the base is 1 to 5wt% of the total amount of phenol; the medium-weak acid includes one or more of organic fatty acids, benzoic acids and phosphoric acid.

[0024] More preferably, in S3, during the process of preparing the thermosetting resin, the alkali is one or a mixture of sodium hydroxide, sodium carbonate and ammonia water; the medium-weak acid is one or a mixture of acetic acid and formic acid.

[0025] Among them, in said S3, the specific steps of preparing the thermoplastic resin are: start stirring, add the p-isopropylphenol / p-propylphenol / 2,3-methylethylphenol obtained by dehydration and stratification after the phenolic resin synthesis in S2 into the reactor; add the m-isopropylphenol / m-p-propylphenol / 2,3-methylethylphenol obtained in S1 in batches, and the first addition is 60-100% of the total amount used; then add acid and perform the first addition of aldehyde;

[0026] After the feeding is completed, the pH of the reaction liquid is measured to be 1-2 with pH test paper, the reflux and venting devices are adjusted, the steam valve is opened to increase the temperature, the steam pressure should not exceed 0.5Mpa, and the heating rate is strictly controlled within 1-3℃ / min; the temperature is raised to 95℃, and the heat preservation reaction is started. The reaction temperature is controlled at 95-100℃ and the heat preservation reaction is carried out for 1-3 hours; then the remaining aldehyde and m-isopropylphenol / m-p-propylphenol / 2,3-methylethylphenol are added for the second time within 1 hour to continue the reaction;

[0027] Pay close attention to the whitening time during the reaction. Add 30-38% hydrochloric acid after 0.5 hours of whitening and continue to keep warm for 1.0 hours.

[0028] Adjust the vacuum device and start vacuum dehydration. The dehydration temperature is controlled at 80-85°C and the final pressure is controlled at -0.075-0.08Mpa. At the same time, observe the water level of the receiver. The water level is generally controlled at 50% of the phenol feed amount. The specific water level is based on the water level being constant within 20 minutes.

[0029] Continue dehydration, control the final pressure at -0.09 to -0.095 MPa, and control the final temperature at 110 to 150°C for 1 to 2 hours of dehydration to make the moisture content meet the requirements. Discharge the material while hot into a stainless steel plate, cool it, and then break it or directly granulate it with a granulator to obtain the thermoplastic resin.

[0030] Preferably, in S3, in the process of preparing the thermoplastic resin, the acid includes one or a mixture of organic fatty acids, benzoic acids, benzenesulfonic acids and inorganic acids; the amount of the acid is 0.1 to 3 wt% of the weight of phenol; the aldehyde includes one or a mixture of fatty aldehydes or benzaldehyde; the amount of the aldehyde is 0.65 to 0.95 of the molar amount of phenol.

[0031] More preferably, in S3, during the process of preparing the thermoplastic resin, the acid is oxalic acid or an oxalic acid / phosphoric acid mixture; the mass ratio of oxalic acid to phosphoric acid in the oxalic acid / phosphoric acid mixture is (7-10):1.

[0032] More preferably, in S3, during the preparation of the thermoplastic resin, the aldehyde is added twice, with 60-70% of the total amount of the aldehyde being added for the first time and 30-40% of the total amount of the aldehyde being added for the second time; the aldehyde is formaldehyde or paraformaldehyde or a mixture of several thereof.

[0033] Beneficial effects: Compared with the prior art, the present invention has the following advantages:

[0034] 1. The present invention utilizes the difference in the reaction activity between the m-isopropylphenol / m-p-propylphenol mixture and formaldehyde to directly produce high-content, high-price m-propylphenol-formaldehyde resin, which can be used as a film material for photoresist; unreacted p-isopropylphenol, p-propylphenol, 2,3-methylethylphenol, etc. are evaporated and distilled to produce high-quality products, so the process is simple, the operation is convenient, the added value is high, and the waste is comprehensively utilized.

[0035] 2. The present invention only needs to selectively control the contents of 2,4-methylethylphenol, 2,3,6-trimethylphenol and 2,4,5-trimethylphenol in meta-p-isopropylphenol / p-propylphenol within the permissible range, and the presence of 2,3-methylethylphenol, 3,4-xylenol, 3-methyl-5-ethylphenol, 2,3,5-trimethylphenol and 3,4-methylethylphenol will not affect the quality of meta-propylphenol-formaldehyde resin. The present invention only needs a few simple steps of resin synthesis, separation of p-isopropylphenol / p-propylphenol / 2,3-methylethylphenol and resin dehydration, with low equipment investment, common equipment, simple and easy-to-control process, less three wastes, short process separation cycle and large output, and directly obtains high value-added products required by the market, so the economic benefits are good.

[0036] 3. The preferred acidic catalysts for the synthesis of the meta-propanol-formaldehyde resin of the present invention are oxalic acid and formic acid. Formic acid can be evaporated, and oxalic acid decomposes into carbon dioxide and water at high temperature. Therefore, the synthesized meta-propanol-formaldehyde resin has better electrical properties, thermal properties, softening point, resolution, etc.

[0037] 4. The raw material of the present invention can also be used for the production of common thermosetting and thermoplastic phenolic resins. Since most of the 2,4-methylethylphenol, 2,3,6-trimethylphenol and 2,4,5-trimethylphenol impurities that affect polymerization are removed, the quality of the produced product is better than that of the same type of phenolic resin produced by commercially available cresol, xylenol and cresol, so that large-scale industrial production can be carried out.

[0038] 5. The by-product p-isopropylphenol / p-propylphenol / 2,3-methylethylphenol mixture of the present invention can be separated by an alkylation method to obtain 2,3-methylethylphenol, antioxidant 2,6-di-tert-butyl-p-isopropylphenol / 2,6-di-tert-butyl-p-propylphenol and other products. Since the content of 2,3-methylethylphenol in crude phenol is significantly lower than that of m-p-isopropylphenol, and the reaction rate of 2,3-methylethylphenol with formaldehyde is twice that of p-isopropylphenol and p-propylphenol, the p-isopropylphenol / p-propylphenol / 2,3-methylethylphenol mixture can be purified to obtain p-isopropylphenol / p-propylphenol.

[0039] 6. The present invention is also applicable to the reaction of m-isopropylphenol and formaldehyde to generate m-isopropylphenol-aldehyde resin, with 98% of p-isopropylphenol as by-product; and is also applicable to the reaction of m-propylphenol and formaldehyde to generate m-propylphenol-aldehyde resin, with 98% of p-propylphenol as by-product. DETAILED DESCRIPTION

[0040] The experimental methods described in the following examples are conventional methods unless otherwise specified; the reagents and materials described are commercially available unless otherwise specified.

[0041] Embodiment 1:

[0042] 1. Distillation, impurity removal and purification of phenol distillation residue

[0043] Attached is the chromatographic analysis report of crude phenol distillation residue (238℃ fraction, crude phenol extracted from low-temperature phenol-containing coal tar in the raw material)

[0044]

[0045]

[0046] 10,000 parts of the crude phenol distillation residue are added to the bottom of a distillation tower, 60 parts of 98% sulfuric acid are added, the temperature is raised to 110-150°C, and then vacuum distillation is performed (vacuum degree -0.088MPa, reflux ratio 25-30:1, tower top temperature 155-185°C), and the contents of various phenols are analyzed by sampling every hour. The front fraction with a mixed content of m-p-isopropylphenol / m-p-propylphenol / 2,3-methylethylphenol ≤50% is collected; then Then collect the m-isopropylphenol / m-propylphenol / 2,3-methylethylphenol fraction; when 3-ethyl-5-methylphenol ≥50%, change to crude 3-methyl-5-ethylphenol; when 2,3,5-trimethylphenol ≥50%, change to crude 2,3,5-trimethylphenol; when 3,4-methylethylphenol ≥50%, change to crude 3,4-methylethylphenol; when 3,4-methylethylphenol ≤40%, stop collecting crude 3,4-methylethylphenol, cool down, and stop distillation. The composition of each fraction is as follows:

[0047]

[0048]

[0049] Notes: (1) 205.2 parts of kettle residue (including 98.8 parts of 3,4-methylethylphenol);

[0050] (2) The front fraction has a complex composition, with high contents of 2,4,6-trimethylol, 2,3,6-trimethylol, 2,4,5-trimethylol, and 2,4 / 2,5-methylethylphenol. It cannot be used to synthesize phenolic resins, but can be used as a solvent for wire enamels.

[0051] (3) The content of 2,4,6-trimethylphenol, 2,3,6-trimethylphenol, 2,4,5-trimethylphenol and 2,4 / 2,5-methylethylphenol in the meta-isopropylphenol / meta-propylphenol / 2,3-methylethylphenol fraction is low and will not affect the synthesis of phenolic resin; the content of meta-isopropylphenol / meta-propylphenol / 2,3-methylethylphenol is 79.12%, meta-isopropylphenol / meta-propylphenol: para-isopropylphenol / para-propylphenol / 2,3-methylethylphenol=43.6:56 .4, in the range of 30-70:70-30, the ratio is good, which can not only synthesize phenolic resin, but also extract p-isopropylphenol, a mixture of p-isopropylphenol and p-propylphenol, etc.; this fraction also contains a large amount of 3-methyl-5-ethylphenol and 2,3,5-trimethylphenol. The thermal stability and optical properties of the phenolic resin synthesized by m-p-isopropylphenol / m-p-propylphenol mixed with 3-methyl-5-ethylphenol and 2,3,5-trimethylphenol will be greatly improved;

[0052] (4) Crude 3-methyl-5-ethylphenol, crude 2,3,5-trimethylphenol, and crude 3,4-methylethylphenol are used to extract high-purity pharmaceutical and material intermediates 3-methyl-5-ethylphenol, 2,3,5-trimethylphenol, and 3,4-methylethylphenol.

[0053] 2. Resin synthesis

[0054] Put 1000 parts of the meta-isopropylphenol / meta-propylphenol fraction obtained by the previous distillation, 7 parts of oxalic acid (15 parts dissolved in water), and 3.5 parts of formic acid into the reactor. After the feeding is completed, start stirring, use pH test paper to determine that the pH of the reaction liquid is 4, adjust the reflux and venting devices, open the steam valve to increase the temperature, the steam pressure should not exceed 0.3Mpa, and gradually add 450 parts of formaldehyde at 90°C. The dropping time is 5 hours, and the temperature is slowly increased after the dropping is completed; the heating rate is strictly controlled within 1-2°C / min, and the rate is determined to be 1.5°C / min, so as to avoid excessive heating, which may cause the reaction liquid to bubble out and affect the resin quality;

[0055] The temperature was raised to 95°C and the reaction was started by heat preservation. The reaction temperature was controlled at 95-100°C and stabilized at 98-100°C. After heat preservation for 2 hours, sampling and analysis were performed. Liquid chromatography analysis showed that 0.26% of meta-isopropylphenol and meta-propylphenol were qualified.

[0056] Steam is introduced for steam distillation to remove free p-isopropylphenol / p-propylphenol / 2,3-methylethylphenol in the material, and no obvious oily matter is observed in the evaporated condensate. When no obvious oily matter is observed in the condensate, the removal of free p-isopropylphenol / p-propylphenol / 2,3-methylethylphenol in the material is completed, and the temperature is slightly lowered; the distillate is separated into layers, and the lower layer is crude p-isopropylphenol / p-propylphenol / 2,3-methylethylphenol. The water layer is extracted twice with toluene (300 parts each time), and the crude p-isopropylphenol / p-propylphenol / 2,3-methylethylphenol layer is combined with the toluene layer, and 591 parts of toluene are obtained by atmospheric distillation, and then reduced pressure distillation is performed to obtain 269.6 parts of 99.3% p-isopropylphenol / p-propylphenol / 2,3-methylethylphenol (162.7 parts of p-isopropylphenol, 50.7 parts of p-propylphenol, and 54.2 parts of 2,3-methylethylphenol).

[0057] After removing free p-isopropylphenol / p-propylphenol / 2,3-methylethylphenol, adjust the vacuum device and start vacuum dehydration. The dehydration temperature is controlled at 80-85°C, the time is controlled at 2-3 hours, and the final pressure is controlled at -0.075-0.08Mpa. At the same time, observe the water level of the receiver. The water level is generally at 370-380 parts. The specific water level shall be constant within 20 minutes.

[0058] The temperature was further increased for dehydration. When the temperature of the material in the kettle reached 200°C and no liquid was distilled out, the temperature was kept for 1 hour, the dehydration was stopped, the vacuum was released with nitrogen, and the material was discharged into a stainless steel plate while hot under nitrogen protection, cooled, crushed and bagged to obtain 784.1 parts of m-propanol-formaldehyde resin in off-white to light yellow color.

[0059] The 99.3% p-isopropylphenol / p-propylphenol / 2,3-methylethylphenol obtained by distillation can be separated by alkylation to produce antioxidant 2,6-di-tert-butyl p-isopropyl / p-propylphenol and 99% 2,3-methylethylphenol.

[0060] Embodiment 2:

[0061] In a reaction kettle, add 81 parts of the dehydrated layered p-isopropylphenol / p-propylphenol / 2,3-methylethylphenol mixture of the above batch of meta-propyl thermosetting phenolic resin in Example 1, add 400 parts of the intermediate p-isopropylphenol / m-p-propylphenol fraction in Example 1 and 30 parts of 25% ammonia water, stir evenly, raise the temperature to about 70-75°C, turn off the steam, slowly raise the temperature to 90-95°C, turn on the cooling water, add 500 parts of 37% formaldehyde dropwise for 4 hours, add the remaining 100 parts of m-isopropylphenol / m-p-propylphenol fraction after the dropwise addition, and continue to keep warm for 2 hours.

[0062] After the reaction is completed, add glacial acetic acid for neutralization, maintain neutrality for 10 minutes and judge it as qualified, then start the vacuum pump to evacuate, start dehydration after the vacuum is stable, observe the dehydration speed slows down or until the temperature drops to about 70-75°C, open the jacket for steam heating, and during dehydration, the steam switch should be continuously adjusted according to the speed of water output to complete the dehydration at a lower temperature as much as possible. Specifically, the temperature is controlled below 75°C in the early stage of dehydration, and steam can be continuously passed after the water output slows down, and the final temperature of the liquid is controlled at about 90°C. When the water level is about (420 parts), samples are taken for analysis of water content and viscosity, and vacuumization is stopped when the water content is 2-3%, and ethylene glycol is added to adjust the viscosity to the specified value of 15-20 Pa.s.

[0063] After the viscosity reaches the requirement, the temperature is lowered to 50°C and 631 parts of the material are discharged. The material is a yellow to light red transparent liquid, and the thermosetting phenolic resin is obtained.

[0064] The separated water was allowed to stand for 1 hour to separate into layers, and 81.3 parts of p-isopropylphenol / p-propylphenol / 2,3-methylethylphenol were obtained for application. The separated water layer was sent to the three waste workshop for treatment.

[0065] Embodiment 3:

[0066] Start stirring in the reactor, add 1000 parts of the intermediate p-isopropylphenol / m-p-propylphenol fraction of Example 1, 158 parts of the p-isopropylphenol / p-propylphenol / 2,3-methylethylphenol mixture recovered from the upper water layer, 8 parts of oxalic acid (dissolved in 16 parts of water), 1 part of phosphoric acid, and 430 parts of 37% formaldehyde.

[0067] After the feeding is completed, use pH test paper to determine the pH of the reaction liquid to be 1-2, adjust the reflux and venting devices, open the steam valve to increase the temperature, the steam pressure should not exceed 0.5Mpa, and the heating rate is strictly controlled within 1-3℃ / min. The rate is determined to be 1.5-2℃ / min to avoid heating too fast, which will cause the reaction liquid to bubble out and affect the resin quality.

[0068] The temperature was raised to 95°C and the heat preservation reaction was started. The reaction temperature was controlled at 95-100°C and stabilized at 98°C. After the heat preservation reaction for 1 hour, the remaining 210 parts of 37% formaldehyde were added dropwise within 1 hour to complete the heat preservation reaction.

[0069] During the reaction, pay close attention to the whitening time. After whitening for 0.5 hours, add 4 parts of 36% hydrochloric acid and continue to keep warm for 1.0 hours. Take samples and observe whether the samples can be stably drawn to end the reaction.

[0070] Adjust the vacuum device and start vacuum dehydration. The dehydration temperature is controlled at 80-85°C and the final pressure is controlled at -0.075-0.08Mpa. At the same time, observe the water level of the receiver. The water level is generally around 490 parts, and the specific water level is based on whether it is constant within 20 minutes. Then gradually increase the vacuum degree to -0.09-0.095Mpa, and distill to a liquid temperature of 130°C for about 1-2 hours. Discharge the material while hot into a stainless steel plate, cool it, and then break it to obtain 1096 parts of light yellow to yellow small pieces of transparent solid, which is thermoplastic resin.

[0071] The evaporated water layer obtained 158.2 parts of a mixture of p-isopropylphenol / p-propylphenol / 2,3-methylethylphenol (p-isopropylphenol / p-propylphenol / 2,3-methylethylphenol content 98.5%), and the water layer was sent to the three wastes treatment section.

[0072] Embodiment 4:

[0073] Put 1000 parts of m-para-isopropylphenol (560 parts of m-isopropylphenol, 440 parts of p-isopropylphenol) obtained by isopropylation of phenol, 7 parts of oxalic acid (15 parts dissolved in water), and 3.5 parts of formic acid into the reactor. After the feeding is completed, start stirring. Use PH test paper to determine that the pH value of the reaction liquid is 4. Adjust the reflux and venting devices, open the steam valve to increase the temperature, the steam pressure should not exceed 0.3Mpa, and gradually add 480 parts of formaldehyde at 90°C. The dropping time is 8 hours, and the temperature is slowly increased after the dropping is completed. The heating rate is strictly controlled within 1-2°C / min, and the rate is determined to be 1.5°C / min to avoid excessively fast heating, which will cause the reaction liquid to bubble out and affect the resin quality.

[0074] The temperature was raised to 95°C and the heat preservation reaction was started. The reaction temperature was controlled at 95-100°C and stabilized at 98-100°C. The sample was analyzed after heat preservation for 4 hours. The liquid chromatography analysis showed that the m-isopropylphenol content was 0.16%, which was qualified.

[0075] The temperature was raised for distillation. After observing that there was no obvious oily substance in the condensate, the temperature was slightly lowered. The distillate was separated into layers, and the lower layer was crude p-isopropylphenol. The aqueous layer was extracted twice with toluene (300 parts each time). The material layer was combined with the toluene layer, and 589 parts of toluene were obtained by atmospheric distillation. Then, 223.8 parts of 99.1% p-isopropylphenol were obtained by vacuum distillation.

[0076] After removing free isopropylphenol, adjust the vacuum device and start vacuum dehydration. The dehydration temperature is controlled at 80-85°C, the time is controlled at 2-3 hours, and the final pressure is controlled at -0.075-0.08Mpa. At the same time, observe the water level of the receiver. The water level is generally at 400-410 parts. The specific water level shall be constant within 20 minutes.

[0077] The temperature was further increased for dehydration. When the temperature of the material in the kettle reached 200°C and no liquid was distilled out, the temperature was kept for 1 hour, the dehydration was stopped, the vacuum was released with nitrogen, and the material was discharged into a stainless steel plate while hot under nitrogen protection, cooled, crushed and bagged to obtain 830.5 parts of m-propanol-formaldehyde resin in off-white to light yellow color.

[0078] The present invention provides a method for preparing phenolic resin by using phenolic distillation residue. There are many methods and ways to implement the technical solution. The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the protection scope of the present invention. All components not specified in this embodiment can be implemented by existing technologies.

Claims

1. A method for preparing phenolic resin using phenolic distillation residue, characterized in that: The specific steps are as follows: S1. distilling and separating the phenol distillation residue to obtain m-isopropylphenol / m-propylphenol / 2,3-methylethylphenol raw materials; S2. Add aldehydes to the meta-isopropylphenol / meta-propylphenol / 2,3-methylethylphenol raw materials obtained in S1, and then steam distill to remove free phenol; the material from which free phenol is removed is heated and decompressed to obtain meta-propylphenol-formaldehyde resin; S3. preparing a thermosetting resin or a thermoplastic resin by using the p-isopropylphenol / p-propylphenol / 2,3-methylethylphenol obtained by dehydrating the water layer in the phenolic resin synthesis in S2; The phenolic distillation residue includes one of a xylenol distillation residue and a crude phenol distillation residue.

2. The method according to claim 1, characterized in that The specific steps of S1 are: adding phenol distillation residue into a reaction kettle, heating to 110-150° C., adding concentrated sulfuric acid dropwise for treatment, subjecting the material to vacuum distillation after treatment, and obtaining m-isopropylphenol / m-propylphenol / 2,3-methylethylphenol raw materials at the top of a distillation tower after reflux dehydration.

3. The method according to claim 2, characterized in that In S1, the amount of concentrated sulfuric acid added is 0.2-1 wt% of the phenol distillation residue.

4. The method according to claim 1, characterized in that: The specific steps of S2 are: mixing the meta-isopropylphenol / meta-propylphenol / 2,3-methylethylphenol raw materials separated in S1 with a catalyst, heating to 80-100° C. and adding aldehydes for reaction, adding for 4-6 hours, keeping warm for 1-2 hours, sampling and analyzing, removing free phenol in the material by steam distillation when the content of meta-isopropylphenol / meta-propylphenol is lower than 0.5%, allowing the distillate to stand to separate the oil layer, extracting the water layer and combining it with the oil layer to obtain an organic layer, distilling the organic layer to obtain a solvent, and further distilling to obtain one or more mixtures of p-isopropylphenol, p-propylphenol and 2,3-methylethylphenol; After the free phenol is evaporated, the material is heated and decompressed to dehydrate, the temperature is raised to 190-200°C, the heating time is 2-3 hours, and then kept warm for 1-2 hours. The vacuum is broken with nitrogen, and the material is discharged into a stainless steel material tray while hot under nitrogen protection to obtain the meta-propanol-formaldehyde resin product.

5. The method according to claim 4, characterized in that In S2, the catalyst includes a mixture of one or more of oxalic acid, formic acid, phosphoric acid, benzoic acid and benzenesulfonic acid; the amount of the catalyst is 0.1 to 5 wt% of the m-isopropylphenol / m-propylphenol / 2,3-methylethylphenol raw materials; the aldehydes include one or more of polyformaldehyde, formaldehyde and acetaldehyde; the amount of the aldehydes is 0.5 to 0.9 of the molar amount of phenol; the solvent is a non-water-soluble solvent, including one of benzene, chlorinated hydrocarbons, chlorinated benzenes, ethers, ketones and esters.

6. The method according to claim 1, characterized in that In the S3, the specific steps of preparing the thermosetting resin are: adding the p-isopropylphenol / p-propylphenol / 2,3-methylethylphenol obtained by dehydrating the water layer after the phenolic resin synthesis in S2 into the reaction kettle; adding the m-isopropylphenol / m-p-propylphenol / 2,3-methylethylphenol obtained in S1 in batches, and the first addition uses 60-100% of the total amount; then adding alkali, turning on the jacket steam heating, raising the temperature to about 50-75°C, turning off the jacket steam, and then slowly raising the temperature to 80-95°C, turning on the cooling water, and adding aldehydes in batches for reaction, the dropping time is 2-4 hours, and then adding the remaining m-isopropylphenol / m-p-propylphenol / 2,3-methylethylphenol raw materials for the second time, and keeping the temperature for reaction for 1-3 hours; After the reaction is completed, a medium or weak acid is added to neutralize to neutrality, and a vacuum pump is turned on for dehydration. When the dehydration speed is observed to slow down or the temperature drops to about 70-75° C., steam heating is turned on to control the final temperature of the liquid at 80-90° C. until the water level is dehydrated to 80% of the mass of the phenolic material, and samples are taken for analysis of water content and viscosity. When the water content is 2-3%, vacuuming is stopped, and the viscosity is adjusted to a specified value of 15-20 Pa.s. After the viscosity reaches the required value, the temperature is lowered to 50° C. and the material is discharged to obtain the thermosetting resin.

7. The method according to claim 6, characterized in that In S3, the base in the process of preparing the thermosetting resin includes one or more of alkali metal hydroxides, alkaline earth metal hydroxides, carbonates, bicarbonates, ammonia water, alcoholamines and hydroxylamines; the amount of the base is 1 to 5wt% of the total amount of phenol; the medium and weak acid includes one or more of organic fatty acids, benzoic acids and phosphoric acid.

8. The method according to claim 1, characterized in that In said S3, the specific steps of preparing the thermoplastic resin are: adding the p-isopropylphenol / p-propylphenol / 2,3-methylethylphenol obtained by dehydration and stratification after the phenolic resin synthesis in S2 in a reaction kettle with stirring; adding the m-isopropylphenol / m-p-propylphenol / 2,3-methylethylphenol obtained in S1 in batches, with the first addition accounting for 60-100% of the total amount used; then adding acid and performing the first addition of aldehyde; After the feeding is completed, the pH of the reaction liquid is controlled to be 1-2, and the steam valve is opened to increase the temperature. The steam pressure should not exceed 0.5Mpa, and the heating rate is controlled within 1-3℃ / min; the temperature is raised to 95℃, and the heat preservation reaction is started for 1-3hr, and the reaction temperature is controlled at 95-100℃; then, aldehyde and the remaining m-isopropylphenol / m-propylphenol / 2,3-methylethylphenol raw materials are added for the second time within 1hr to continue the reaction; when the reaction turns white, 30-38% hydrochloric acid is added after 0.5hr, and the heat preservation is continued The reaction was carried out for 1.0 hour; vacuum dehydration was carried out, the dehydration temperature was controlled at 80-85°C, the final pressure was controlled at -0.075-0.08Mpa, when the water level of the receiver was about 50% of the phenol feed amount and the water level was constant within 20 minutes, the vacuum degree was increased to -0.09-0.095Mpa, the final temperature of dehydration was controlled at 110-150°C for 1-2 hours, the material was discharged while hot into a stainless steel plate, and then crushed after cooling or directly granulated by a granulator to obtain the thermoplastic resin.

9. The method according to claim 8, characterized in that In S3, in the process of preparing the thermoplastic resin, the acid includes one or a mixture of organic fatty acids, benzoic acids, benzenesulfonic acids and inorganic acids; the amount of the acid is 0.1 to 3 wt% of the weight of phenol; the aldehyde includes one or a mixture of fatty aldehydes or benzaldehyde; the amount of the aldehyde is 0.65 to 0.95 of the molar amount of phenol.

10. The method according to claim 9, characterized in that In S3, during the preparation of the thermoplastic resin, the aldehyde is added twice, with the first addition accounting for 60-70% of the total amount of the aldehyde and the second addition accounting for 30-40% of the total amount of the aldehyde.

Citation Information