Chemical oxidation resistant polishing pad and preparation method and application thereof
By using chemical oxidation-resistant polishing pads prepared with materials such as polyurethane prepolymers, combined with precuring and corona treatment technology, the problem of low service life and efficiency of existing polishing pads under high temperature and high pressure conditions is solved, and higher polishing is achieved Rate and service life are suitable for the processing needs of SiC substrates.
Patent Information
- Application Number
- CN202411156349.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-22
AI Technical Summary
In existing SiC chemical mechanical polishing, the polishing pad has low service life and polishing efficiency under high temperature, high pressure and strong oxidation conditions, making it difficult to meet the production needs of the new generation of SiC power devices.
The chemical oxidation-resistant polishing pad is formed by using raw materials such as polyurethane prepolymer, bisphenol A epoxy phenolic copolymer, chain extender and foaming agent, and the impact strength is improved through precuring, post-curing and corona treatment processes. , chemical oxidation resistance and polishing properties.
It significantly improves the service life and polishing rate of the polishing pad, enhances the processing performance of silicon carbide substrates, and shows high compatibility and stability in highly corrosive polishing liquid, which is suitable for large-scale industrial production.
Smart Images

Figure BDA0005005085600000111 
Figure BDA0005005085600000121 
Figure BDA0005005085600000122
Abstract
Description
Technical Field
[0001] The invention relates to the field of materials for polishing pads, and in particular to a chemical oxidation resistant polishing pad and a preparation method and application thereof. Background Art
[0002] In order to achieve the full popularization of the new generation of SiC power devices, the large-diameter mass production of substrates is being continuously promoted, and the importance of substrate processing technology is also increasing. At present, chemical mechanical polishing (CMP) is widely used internationally to obtain ultra-smooth, damage-free silicon carbide substrate surfaces. CMP technology is a technology that rotates the polishing workpiece relative to the polishing pad under a certain pressure, and uses the mechanical grinding of abrasive particles and the chemical corrosion of chemical additives to remove materials from the workpiece surface under the action of a flowing polishing liquid medium (a mixture of abrasive particles, various chemical additives and solvents), thereby achieving global flattening of the workpiece surface.
[0003] In the SiC chemical mechanical polishing (CMP) process, the chemical action is provided by the oxidant component in the polishing liquid, which is usually a strong oxidizing component such as potassium ferrate and potassium permanganate. The effective proportion can be as high as 5%. The service life and polishing efficiency of the polishing pad are seriously damaged under this high temperature, high pressure and strong oxidizing polishing condition. Summary of the invention
[0004] In view of the above-mentioned shortcomings of the prior art, an object of the present invention is to provide a chemical oxidation resistant polishing pad and a preparation method and use thereof, so as to solve the problems in the prior art.
[0005] To achieve the above objectives and other related objectives, the present invention is achieved through the following technical solutions.
[0006] The invention provides a chemical oxidation resistant polishing pad, which comprises the following raw material components: a polyurethane prepolymer, a bisphenol A epoxy phenolic copolymer, a chain extender and a foaming agent.
[0007] Preferably, the raw material components include the following parts by weight:
[0008] Polyurethane prepolymer 90-110 parts
[0009] 2.5-15 parts of bisphenol A epoxy novolac copolymer
[0010] Chain extender 30-70 parts
[0011] Foaming agent 0.05~2 parts.
[0012] For example, the amount of polyurethane prepolymer used can be 90-100 parts or 100-110 parts.
[0013] For example, the amount of bisphenol A epoxy novolac copolymer can be 2.5 to 4 parts, 4 to 4.4 parts, 4.4 to 5, 5 to 10 parts, 10 to 15 parts, preferably 5 to 15 parts, more preferably 10 to 15 parts. When the amount of bisphenol A epoxy novolac copolymer is reduced, appropriately increasing the amount of polyether diol will not weaken the polishing effect of the polishing pad.
[0014] For example, the amount of polyether diol used can be 10-11 parts, 11-20 parts, 20-22 parts, or 22-30 parts.
[0015] For example, the amount of the chain extender can be 30-32 parts, 32-35 parts, 35-42 parts, 42-45 parts, 45-55 parts, 55-62 parts, 62-65 parts, or 65-70 parts.
[0016] For example, the amount of the foaming agent can be 0.05-0.1 parts, 0.1-1 parts, or 1-2 parts.
[0017] Preferably, the Shore hardness of the polyurethane prepolymer is 73-75HD.
[0018] Preferably, the content of isocyanate groups in the polyurethane prepolymer is 9.4-9.7 wt %.
[0019] Preferably, the polyurethane prepolymer is prepared by reacting polyether diol and toluene diisocyanate.
[0020] Preferably, the bisphenol A epoxy novolac copolymer is obtained by copolymerizing a bisphenol A epoxy prepolymer and a phenolic condensation polymer.
[0021] More preferably, the raw materials of the bisphenol A type epoxy prepolymer include bisphenol A and epichlorohydrin.
[0022] More preferably, the phenolic condensation polymer is a novolac condensation polymer.
[0023] More preferably, the mass ratio of the bisphenol A epoxy prepolymer to the phenolic condensation polymer is (7-30):3, such as 7:3, 10:3, 5:1, 20:3, 25:3, 9:1, 10:1.
[0024] More preferably, the copolymerization reaction uses a curing accelerator, and more preferably, the curing accelerator is N,N-dimethylbenzylamine.
[0025] More preferably, the reaction temperature of the copolymerization is 150-160°C.
[0026] More preferably, the copolymerization reaction time is 1 to 2 hours.
[0027] More preferably, the bisphenol A epoxy prepolymer has an epoxy equivalent of 171-175 g / eq and a viscosity of 4000-6000 mPa·s at 25°C.
[0028] More preferably, the phenolic polycondensate has a viscosity of 350-450 mPa·s at 25°C.
[0029] More preferably, the non-volatile matter content of the phenolic polycondensate at 135° C. is 70-80%.
[0030] Preferably, the chain extender is 3,5-diethyltoluenediamine and / or 3,3'-dichloro-4,4'-diphenylmethanediamine.
[0031] Preferably, the blowing agent is water.
[0032] Preferably, the raw material components further include polyether diol.
[0033] More preferably, the amount of the polyether diol used is 10 to 30 parts.
[0034] More preferably, the polyether diol is polytetramethylene ether diol.
[0035] Preferably, the raw material components further include a catalyst, and the catalyst includes triethylenediamine. The catalyst is used to stabilize the balance between the foaming rate and the gelling rate.
[0036] More preferably, the amount of the catalyst is 0.03 to 0.2 parts, such as 0.03 to 0.1 parts, or 0.1 to 0.2 parts.
[0037] More preferably, in the catalyst, the content of triethylenediamine is 30-35wt%. For example, in the catalyst, the content of triethylenediamine can be 30-33wt%, 33-35wt%.
[0038] More preferably, the catalyst further comprises a diol, and the diol is selected from one or more of dipropylene glycol, butanediol and ethylene glycol.
[0039] Preferably, the raw material components further include a surfactant, which is used to increase the mutual solubility between components, stabilize the slurry foam, and adjust the pores of the chemical oxidation resistant polishing pad.
[0040] More preferably, the amount of the surfactant is 1 to 5 parts, such as 1 to 2 parts, 2 to 3 parts, 3 to 4 parts, or 4 to 5 parts.
[0041] More preferably, the surfactant is one or more selected from linear polysiloxane, polydimethylsiloxane and polysiloxane-oxyalkylene block copolymer.
[0042] Further preferably, the surfactant is silicone oil and / or organosilicon surfactant
[0043] More preferably, the surfactant is selected from Dow DC-193 and / or Momentive Niax L-1500.
[0044] Preferably, the chemical oxidation resistant polishing pad comprises one or more of the following characteristics: Shore hardness of 45-70 HD, density of 0.5-0.8 g / cm 3 The compression rate is 0.9-2.0%, the compression elasticity is 55-80%, the tensile strength is 4.5-8.5Mpa, and the elongation at break is 180-230%.
[0045] Preferably, the chemical oxidation resistant polishing pad is immersed in a 5.0wt.% potassium permanganate solution, immersed in a sealed container at 50±1°C for 24 hours, and after cleaning and drying, the thickness of the chemical corrosion layer formed by oxidation on the side section is observed under an optical microscope to be less than 600μm. For example, it can be 555μm, 501μm, 433μm, 423μm, 400μm, 356μm, 261μm, 243μm, 240μm.
[0046] Preferably, the chemical oxidation resistant polishing pad is abraded by an H-18 ceramic grinding wheel with a load of 1000g, rotates at a speed of 75rpm, and the mass loss after 100 revolutions is not higher than 130mg, the mass loss after 500 revolutions is not higher than 180mg, and the mass loss after 1000 revolutions is not higher than 240mg. For example, the mass loss after 100 revolutions can be 126.1mg, 100.7mg, 95.1mg, 88.9mg, 80.1mg, 79.3mg, 77.4mg, 61mg, 60.6mg. For example, the mass loss after 500 revolutions can be 177.5mg, 165.9mg, 121.9mg, 110.8mg, 110.7mg, 101.5mg, 100.3mg, 98.5mg, 98.3mg. For example, the mass loss after 1000 rotations can be 235.4 mg, 190.8 mg, 178.9 mg, 150.9 mg, 142.3 mg, 140.2 mg, 132.6 mg, 120.5 mg, and 119.1 mg.
[0047] The present invention also discloses a method for preparing the chemical oxidation resistant polishing pad as described above, wherein the raw material components are uniformly mixed and pre-cured to obtain the chemical oxidation resistant polishing pad.
[0048] Preferably, before mixing, the polyurethane prepolymer, the bisphenol A epoxy novolac copolymer and the polyether diol are preheated and vacuumed.
[0049] More preferably, the preheating temperature is 75-95°C.
[0050] Preferably, the chain extender is preheated before mixing.
[0051] More preferably, the preheating temperature is 90-100°C.
[0052] Preferably, the pre-curing temperature is 75-85°C, more preferably 80°C.
[0053] Preferably, the pre-curing time is 2 to 4 hours.
[0054] Preferably, a post-curing treatment is performed after curing.
[0055] More preferably, the post-curing temperature is 95-105°C, more preferably 100°C.
[0056] More preferably, the post-curing time is 15 to 24 hours, more preferably 16 hours.
[0057] More preferably, the post-curing treatment is followed by slicing, grinding, grooving, surface cleaning and corona treatment.
[0058] By applying high-frequency and high-voltage current to the electrodes, corona discharge is generated at the electrodes, and the gas is ionized to produce high-energy ions, which impact the surface of the material under the action of a strong electric field and change the surface properties of the material.
[0059] Further preferably, the object of the corona treatment is the bonding surface of the polishing pad that contacts the substrate.
[0060] Further preferably, the input voltage of the corona treatment is AC300-400V, the power is 2-70KW, and the electrode gap is 1-2mm. For example, the input voltage may be 300-380V, 380-400V, the power may be 2-25KW, 25-50KW, 50-70KW, and the electrode gap may be 1-1.2mm, 1.2-1.4mm, 1.4-1.6mm, 1.6-1.8mm, 1.8-2.0mm.
[0061] Further preferably, the grinding is to use a grinding wheel to grind the working surface of the chemical oxidation resistant polishing pad.
[0062] The present invention also discloses the use of the chemical oxidation resistant polishing pad as described above as a polishing pad for polishing a SiC substrate in chemical mechanical polishing.
[0063] The present invention provides a chemical oxidation resistant polishing pad and a preparation method and use thereof, which have the following beneficial effects:
[0064] (1) In the preparation of chemical oxidation resistant polishing pads, by adding bisphenol A epoxy phenolic copolymer and adjusting the raw material composition for physical blending, microphase separation occurs during the chemical foaming, cross-linking and curing stage, thereby enhancing the performance of the polyurethane hard segment, improving the impact strength, chemical oxidation resistance and wear resistance, and thus improving the polishing rate and service life;
[0065] (2) The performance of the soft segment of the original polyurethane prepolymer is further enhanced by introducing polyether diol, and the dynamic mechanical properties, hydrolysis resistance, toughness and flexibility of the chemical oxidation resistant polishing pad are comprehensively increased, and the polishing rate and service life of the chemical oxidation resistant polishing pad are further improved;
[0066] (3) The synergistic effect of using bisphenol A epoxy phenolic copolymer and polyether diol is improved, which improves the polishing rate of the chemical oxidation resistant polishing pad and improves the overall polishing performance of the polishing pad; and the polishing pad prepared by using bisphenol A epoxy phenolic copolymer and polyether diol has a longer service life and a higher surface quality of the silicon carbide substrate processing, and has strong compatibility with the matching polishing liquid, which is better than the commercially available polishing pad products;
[0067] (4) In the preparation method, corona treatment is added to the adhesive bonding surface of the polishing pad to induce chemical bond breakage, improve the wettability and adhesion of the polishing pad bonding surface, and enhance the bonding force between the polishing pad and the adhesive, thereby ensuring that the highly corrosive polishing liquid does not debond when it penetrates into the pores between the polishing pad and the adhesive during polishing, and increasing the uniformity of chemical oxidation resistance, thereby improving the stability of the polishing rate;
[0068] (6) The preparation method is simple, the product is highly stable, and is suitable for large-scale industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0069] Figure 1 The thermal analysis test graph of the chemical oxidation resistant polishing pad prepared in Example 5 is shown. DETAILED DESCRIPTION
[0070] The following is a description of the implementation of the present invention by means of specific embodiments. Those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification.
[0071] Before further describing the specific embodiments of the present invention, it should be understood that the scope of protection of the present invention is not limited to the specific embodiments described below; it should also be understood that the terms used in the examples of the present invention are intended to describe specific embodiments, rather than to limit the scope of protection of the present invention. The test methods in the following examples without specifying specific conditions are generally carried out under conventional conditions or under conditions recommended by the manufacturers.
[0072] When the embodiments give numerical ranges, it should be understood that, unless otherwise specified in the present invention, both endpoints of each numerical range and any numerical value between the two endpoints can be selected. Unless otherwise defined, all technical and scientific terms used in the present invention have the same meaning as those generally understood by those skilled in the art. In addition to the specific methods, equipment, and materials used in the embodiments, according to the grasp of the prior art by those skilled in the art and the record of the present invention, any methods, equipment, and materials of the prior art similar or equivalent to the methods, equipment, and materials described in the embodiments of the present invention can also be used to realize the present invention.
[0073] The bisphenol A epoxy novolac copolymer of the present invention is prepared by the following method:
[0074] The phenolic condensation polymer is a linear phenolic condensation polymer, with a viscosity (25°C): 350-450 mPa·s, a non-volatile matter ratio (135°C): 70%, and an epoxy equivalent of the bisphenol A type epoxy prepolymer of 171-175 g / eq and a viscosity of 4000-6000 mPas (temperature 25°C).
[0075] The phenolic polycondensate and the bisphenol A epoxy prepolymer are mixed in a mass ratio of 3:(7-30) and heated to 70-75° C. After the viscosity of the mixture decreases, 1-1.5 wt% of a curing accelerator N,N-dimethylbenzylamine is added to the mixture, and then the mixture is cured at 150-160° C. for 1-2 hours to obtain a fluidized bisphenol A epoxy novolac copolymer, which is stored at room temperature of 25-27° C. under nitrogen protection.
[0076] The specific implementation method of the present invention provides a specific method for preparing a chemical oxidation resistant polishing pad, and the preparation steps are as follows:
[0077] (1) Pretreatment of raw materials:
[0078] Add 90-110 parts of polyurethane prepolymer, 2.5-15 parts of bisphenol A epoxy phenolic copolymer, and 10-30 parts of polytetramethylene glycol into material tank A, stir and blend at a speed of 2500-3000 rpm for 1.5-2 hours, evacuate, and keep warm at 75-85°C;
[0079] Add 0.05-2 parts of deionized water, 0.03-0.2 parts of catalyst and 1-5 parts of silicone surfactant into the S material tank, and stir and blend at 2000-2500 rpm for 5-10 minutes at room temperature;
[0080] Add 30-70 parts of 3,5-diethyltoluenediamine DETDA into the C material tank and keep it warm at 75-85°C.
[0081] The hardness of the polyurethane prepolymer is 73-75HD, and the content of isocyanate groups in the polyurethane prepolymer is 9.4-9.7%.
[0082] (2) Curing
[0083] A, C, and S tanks are mixed and discharged at the same time, with a discharge port speed of 4000-4500rpm. After the discharge, the material is directly poured into a cylindrical mold at 75-85℃. After the mixed slurry is completely poured into the mold, the mold cover is closed, and the mold pressure ratio is 1.0-1.2. The discharge material is kept warm in the mold for 2-4 hours before demoulding the sample block.
[0084] (3) The removed sample is placed in an oven for post-curing treatment for 15 to 24 hours at a post-curing temperature of 95 to 105°C.
[0085] (4) The sample block is sliced, and the working surface of the slice is polished, grooved, surface cleaned, and the bonding surface is corona treated to obtain a chemical oxidation resistant polishing pad with a thickness of 2.00 mm ± 0.05 mm and a surface roughness of 15.05 ± 4.00 μm.
[0086] The following are more specific examples. The reagents used in the following examples are all commonly used reagents and can be purchased from the market, as follows:
[0087] Polyurethane prepolymer, purchased from Covestro, Germany LU-T75D;
[0088] Bisphenol A type liquid epoxy prepolymer was purchased from Dow Chemical, USA, with the brand name DER-332;
[0089] Phenolic polycondensate was purchased from Sumitomo, Japan, model PR-9400;
[0090] Polytetrahydrofuran ether glycol was purchased from BASF PolyTHF 2000, USA;
[0091] 3,5-Diethyltoluenediamine DETDA was purchased from Albemarle, USA, model number 100Curative.
[0092] The catalyst is a solution of 33% triethylenediamine and 67% dipropylene glycol, purchased from Niax A-33 of the United States.
[0093] The organosilicon surfactant was purchased from Momentive, USA, model number is Niax*L-1500.
[0094] The test method for the isocyanate group content in polyurethane prepolymer is: Method A in HG / T 2409-2023.
[0095] The epoxy equivalent of bisphenol A epoxy prepolymer is tested using GB / T 4612-2008.
[0096] Test method for viscosity of bisphenol A epoxy prepolymer: GB / T 22314-2008.
[0097] Test method for viscosity of phenolic condensation polymer: HG / T 2712-1995 "Determination of viscosity of liquid and solution phenolic resins".
[0098] Percentage of non-volatile matter in phenolic condensation polymers: Adopt HG / T 2711-1995 "Routine determination of non-volatile matter in liquid phenolic resins", test temperature 135℃, test time 1h.
[0099] Example 1
[0100] This embodiment provides a more specific chemical oxidation resistant polishing pad, and the preparation method is as follows:
[0101] 1. Preparation of bisphenol A epoxy novolac copolymer:
[0102] The phenolic polycondensate and the bisphenol A epoxy prepolymer were mixed in a mass ratio of 1:9 and heated to 60°C. After the viscosity of the mixture decreased, 1wt% of the mixture mass of a curing accelerator N,N-dimethylbenzylamine was added, and after being fully mixed, the mixture was cured at 150°C for 1h to obtain a fluidized bisphenol A epoxy novolac copolymer. The prepared fluidized bisphenol A epoxy novolac copolymer was stored at room temperature under nitrogen protection for later use.
[0103] 2. Preparation of chemical oxidation resistant polishing pad:
[0104] (1) Pretreatment of raw materials:
[0105] Add 100 parts of polyurethane prepolymer, 2.5 parts of bisphenol A epoxy novolac copolymer, and 22 parts of polytetramethylene glycol into material tank A, evacuate and keep warm at 80°C, and stir and blend at 2500 rpm for 2 hours;
[0106] Add 0.15 parts of deionized water, 0.1 parts of catalyst and 2 parts of silicone surfactant into the S material tank, and stir and blend at 2000 rpm for 5 minutes at room temperature;
[0107] Add 35 parts of 3,5-diethyltoluenediamine DETDA into the C material tank and keep it at 80°C.
[0108] The hardness of the polyurethane prepolymer is 75HD, and the content of isocyanate groups in the polyurethane prepolymer is 9.4-9.7%.
[0109] (2) Curing
[0110] The A, C, and S tanks were mixed and discharged at the same time, with a discharge port speed of 4000rpm. After the discharge, the material was directly poured into a cylindrical mold at 80℃. After the mixed slurry was completely poured into the mold, the mold cover was closed, and the mold pressure ratio was 1.2. The discharge material was pre-cured in the mold for 2 hours before the sample was demoulded.
[0111] (3) The removed sample was transferred to an oven for post-curing for 16 hours at a post-curing temperature of 100°C.
[0112] (4) The sample block is sliced, and the working surface of the slice is polished, grooved, and cleaned. The bonding surface of the polishing pad that is bonded to the substrate is corona treated with a corona treatment machine. The input voltage of the corona treatment is AC380V, the power is 25KW, the electrode gap is 1.2mm, and the thickness of the polishing pad is 2.05mm and the surface roughness is 15.50μm.
[0113] Example 2
[0114] This embodiment provides a more specific chemical oxidation resistant polishing pad, using the bisphenol A epoxy novolac copolymer prepared in Example 1. The preparation method of the chemical oxidation resistant polishing pad is different from that of Example 1 only in that:
[0115] In step (1), the raw material components do not contain polytetrahydrofuran ether glycol;
[0116] In step (4), the thickness of the chemical oxidation resistant polishing pad is 2.01 mm and the surface roughness is 15.40 μm;
[0117] The remaining process steps are the same.
[0118] Example 3
[0119] This embodiment provides a more specific chemical oxidation resistant polishing pad, using the bisphenol A epoxy novolac copolymer prepared in Example 1. The preparation method of the chemical oxidation resistant polishing pad is basically the same as that of Example 1, except that:
[0120] In step (1), the raw material components include 5 parts of bisphenol A epoxy novolac copolymer and 45 parts of 3,5-diethyltoluenediamine DETDA.
[0121] In step (4), the thickness of the chemical oxidation resistant polishing pad is 2.10 mm and the surface roughness is 15.11 μm.
[0122] The remaining process steps are the same.
[0123] Example 4
[0124] This embodiment provides a more specific chemical oxidation resistant polishing pad, using the bisphenol A epoxy novolac copolymer prepared in Example 1. The preparation method of the chemical oxidation resistant polishing pad is different from that of Example 3 only in that:
[0125] In step (1), the raw material components do not contain polytetrahydrofuran ether glycol;
[0126] In step (4), the thickness of the chemical oxidation resistant polishing pad is 2.08 mm and the surface roughness is 15.83 μm.
[0127] The remaining process steps are the same.
[0128] Example 5
[0129] This embodiment provides a more specific chemical oxidation resistant polishing pad, using the bisphenol A epoxy novolac copolymer prepared in Example 1. The preparation method of the chemical oxidation resistant polishing pad is basically the same as that of Example 1, except that:
[0130] In step (1), the raw material components include 10 parts of bisphenol A epoxy novolac copolymer and 65 parts of 3,5-diethyltoluenediamine DETDA.
[0131] In step (4), the thickness of the chemical oxidation resistant polishing pad is 2.11 mm and the surface roughness is 16.00 μm.
[0132] Example 6
[0133] This embodiment provides a more specific chemical oxidation resistant polishing pad, using the bisphenol A epoxy novolac copolymer prepared in Example 1. The preparation method of the chemical oxidation resistant polishing pad is different from that of Example 5 only in that:
[0134] In step (1), the raw material components do not contain polytetrahydrofuran ether glycol;
[0135] In step (4), the thickness of the chemical oxidation resistant polishing pad is 2.00 mm, and the surface roughness is 14.92 μm.
[0136] The remaining process steps are the same.
[0137] Example 7
[0138] This embodiment provides a more specific chemical oxidation resistant polishing pad, using the bisphenol A epoxy novolac copolymer prepared in Example 1. The preparation method of the chemical oxidation resistant polishing pad is different from that of Example 5 only in that:
[0139] In step (1), the amount of bisphenol A epoxy novolac copolymer is 15 parts; the amount of 3,5-diethyltoluenediamine is 85 parts;
[0140] In step (4), the thickness of the chemical oxidation resistant polishing pad is 2.03 mm and the surface roughness is 15.06 μm.
[0141] The remaining process steps are the same.
[0142] Example 8
[0143] This comparative example provides a more specific chemical oxidation resistant polishing pad, using the bisphenol A epoxy novolac copolymer prepared in Example 1. The preparation method of the chemical oxidation resistant polishing pad is different from that of Example 3 only in that:
[0144] In step (1), the amount of polytetrahydrofuran ether glycol is 11 parts;
[0145] In step (4), the thickness of the chemical oxidation resistant polishing pad is 2.07 mm and the surface roughness is 15.09 μm.
[0146] The remaining process steps are the same.
[0147] Example 9
[0148] This comparative example provides a more specific chemical oxidation resistant polishing pad, using the bisphenol A epoxy novolac copolymer prepared in Example 1. The preparation method of the chemical oxidation resistant polishing pad is different from that of Example 1 only in that:
[0149] In step (1), the amount of bisphenol A epoxy novolac copolymer is 4 parts, and the amount of polytetramethylene ether glycol is 15 parts;
[0150] In step (4), the thickness of the chemical oxidation resistant polishing pad is 2.00 mm and the surface roughness is 15.11 μm.
[0151] The remaining process steps are the same.
[0152] Comparative Example 1
[0153] This comparative example provides a more specific chemical oxidation resistant polishing pad, and the preparation method is different from that of Example 5 only in that: in step (1), the raw material components do not contain bisphenol A epoxy novolac copolymer and polytetramethylene glycol;
[0154] In step (4), the thickness of the chemical oxidation resistant polishing pad is 2.13 mm and the surface roughness is 15.05 μm.
[0155] The remaining process steps are the same.
[0156] Comparative Example 2
[0157] This comparative example provides a more specific chemical oxidation resistant polishing pad, and the preparation method is different from that of Example 5 only in that: in step (1), the raw material components do not contain bisphenol A epoxy novolac copolymer;
[0158] In step (4), the thickness of the chemical oxidation resistant polishing pad is 2.06 mm and the surface roughness is 15.57 μm.
[0159] The remaining process steps are the same.
[0160] Comparative Example 3
[0161] This comparative example provides a more specific chemical oxidation resistant polishing pad, and the preparation method is different from that of Example 5 only in that: in step (1), bisphenol A type liquid epoxy prepolymer is used in the raw material components instead of bisphenol A epoxy novolac copolymer.
[0162] In step (4), the thickness of the chemical oxidation resistant polishing pad is 2.11 mm and the surface roughness is 15.61 μm.
[0163] The remaining process steps are the same.
[0164] Comparative Example 4
[0165] This comparative example provides a more specific chemical oxidation resistant polishing pad, and the preparation method is different from that of Example 5 only in that:
[0166] There is no corona surface treatment step for the bonding surface. In step (4), the thickness of the chemical oxidation resistant polishing pad is 2.18 mm and the surface roughness is 15.41 μm.
[0167] The remaining process steps are the same.
[0168] The chemical oxidation resistant polishing pads prepared in Examples 1 to 9 and Comparative Examples 1 to 3 were subjected to the following performance tests: hardness test, compression test, compression elasticity test, mechanical property test and chemical oxidation resistance test. The test results are shown in Table 1.
[0169] The wear resistance of the chemical oxidation resistant polishing pads prepared in Examples 1 to 9 and Comparative Examples 1 to 3 and a commercially available polishing pad (DuPont, IC1000) was tested. The test results are shown in Table 2.
[0170] Polishing rate tests were performed on the chemical oxidation resistant polishing pads prepared in Examples 1 to 9 and Comparative Examples 1 to 4 and a commercially available polishing pad (DuPont, IC1000, USA). The test results are shown in Table 3.
[0171] The chemical oxidation resistant polishing pads prepared in Examples 5 to 6 and Comparative Examples 1 to 4 and a commercially available polishing pad (DuPont, IC1000) were tested for service life. The test results are shown in Table 4.
[0172] Thermal analysis test was performed on Example 5, and the test results are shown in Figure 1 .
[0173] The test method is as follows:
[0174] 1. Hardness test: GB / T 2411-2008;
[0175] 2. Density test: GB / T 6343-2009;
[0176] 3. Compression rate and compression elasticity test:
[0177] A manual thickness gauge was used to measure the light compression thickness T0, heavy compression thickness T1, and recovery thickness T2, and the compression rate and compression elasticity were calculated according to the following formula.
[0178] Compression ratio = (T0-T1) / T0*100%
[0179] Compression elasticity = (T2-T1) / (T0-T1)*100%;
[0180] The units of T0, T1 and T2 are all mm.
[0181] The test methods for light pressure thickness T0, heavy pressure thickness T1, and recovery thickness T2 are as follows:
[0182] (1) Cut 5 specimens of 30 mm × 30 mm from the polishing pad product and condition the specimens in a relaxed state for at least 2 h at standard atmospheric pressure and 25 ± 2 °C;
[0183] (2) Clean the presser foot and lower workbench, put down the presser foot, and reset (the presser foot area is 0.785cm 2 );
[0184] (3) Place the state-adjusted sample flat and tension-free on a workbench, add a 235.5 g weight, maintain pressure for 30 seconds, and record the light pressure thickness T0.
[0185] (4) Add a weight of 1177.5 g again, maintain the pressure for 60 seconds, and then record the thickness T1.
[0186] (5) Immediately remove all weights, lift the presser foot, and allow the sample to recover for 60 seconds before applying a 235.5 g weight again. Maintain the pressure for 30 seconds and measure the thickness under the second light pressure, i.e., the recovered thickness T2.
[0187] 4. Mechanical properties test: GB / T 528-2009 was used to test the tensile strength and elongation at break. Five dumbbell-shaped specimens were used, and the specimen size was type 2. The test results were averaged.
[0188] 5. Chemical oxidation resistance test: Immerse the polishing pad in a 5.0wt.% potassium permanganate solution in a sealed container at 50±1℃ for 24 hours. After cleaning and drying, observe the thickness of the chemical corrosion layer formed by oxidation on the side section under an optical microscope. The smaller the thickness of the chemical corrosion layer, the better the chemical oxidation resistance.
[0189] 6. Wear resistance test: The wear resistance of the polishing pad was measured by a Taber abraser. The polishing pad was cut into samples with a diameter of 108 mm and abraded with an H-18 ceramic grinding wheel with a load of 1000 g. The pad was rotated at 75 rpm and the mass loss (mg) after 100, 300, 500 and 1000 revolutions was recorded.
[0190] 7. Thermal analysis test
[0191] TG-DSC synchronous thermal analyzer, model: NETZSCH STA 449F3;
[0192] Test conditions:
[0193] Heating rate: 10.0K / min, temperature range: 25℃-300℃, test atmosphere: N2. Test results are shown in Figure 1 .
[0194] pass Figure 1 Analysis shows that the chemical oxidation resistant polishing pad prepared in Example 5 has a glass transition temperature of 240° C., and a mass loss of only 6.25% at 300° C., indicating excellent thermal stability.
[0195] 8. Polishing rate test:
[0196] A 6-inch silicon carbide substrate was polished using a polishing machine, and the polishing rate was recorded. Polishing machine table: 915 mm, polishing liquid: Bolinerun COPOL-431 (manganese oxide polishing liquid, pH = 2.7, abrasive manganese oxide particle size 20 nm), polishing liquid flow rate: 400 ml / min, polishing pressure: 300 g / cm 3 , speed 80rpm, polishing method: Si surface polishing, veneering method: solid wax, polishing times: 3 times, polishing time each time: 2h.
[0197] 9. Service life test: A polishing machine was used to test the service life of the polishing pad on a 6-inch silicon carbide substrate. The polishing rate (MRR) and the surface roughness (Ra) of the silicon carbide were recorded after each round of polishing. Once the MRR value was lower than 2μm / h (polishing liquid 1) / 1.35μm / h (polishing liquid 2), or the Ra value was higher than 1nm, polishing was stopped. The total polishing time was the service life (min) of the polishing pad.
[0198] Test conditions: polishing machine: 915mm, polishing liquid 1: Boline COPOL-431 (manganese oxide polishing liquid pH = 2.7, abrasive manganese oxide particle size 20nm), polishing liquid 2: Ferro-SN12500 (Al2O3, pH = 8-10), polishing liquid flow rate: 400ml / min, polishing pressure: 300g / cm 3 , speed 80rpm, polishing method: Si surface polishing, veneering method: adsorption pad, polishing times: based on MRR or Ra value, each polishing time: 20min.
[0199] Table 1
[0200]
[0201]
[0202] Table 2
[0203]
[0204] Table 3
[0205]
[0206]
[0207] Table 4
[0208]
[0209] From Table 1 we can see that:
[0210] It can be seen from the thickness of the chemical corrosion layer in Examples 5-6 and Comparative Examples 1-2 that the bisphenol A epoxy novolac copolymer and the polyether diol synergistically improve the chemical oxidation resistance of the chemical oxidation resistant polishing pad.
[0211] From Tables 2 and 3, we can see that:
[0212] From the comparison of the data of Examples 5 to 6 and Comparative Example 1, it can be seen that the addition of bisphenol A epoxy novolac copolymer to the chemical oxidation resistant polishing pad can greatly improve the polishing rate of the chemical oxidation resistant polishing pad, and the addition of polytetramethylene ether glycol can further improve the polishing rate;
[0213] It can be seen from the data of Examples 5-6 and Comparative Examples 1-2 that the bisphenol A epoxy novolac copolymer and the polyether polyol synergistically improve the polishing rate and wear resistance of the chemical oxidation resistant polishing pad.
[0214] It can be seen from the data of Examples 1, 3, 5 and 7 that when the amount of polytetramethylene ether glycol is constant, when the amount of bisphenol A epoxy novolac copolymer is increased from 2.5 parts to 10 parts, the polishing efficiency increases gradually, and when the amount of bisphenol A epoxy novolac copolymer is increased to 15 parts, the polishing rate changes very little.
[0215] It can be seen from Examples 1 and 9 that when the amount of bisphenol A epoxy novolac copolymer is reduced, appropriately increasing the amount of polytetramethylene ether diol will not weaken the polishing effect of the chemical oxidation resistant polishing pad.
[0216] It can be seen from the data of Example 5 and Comparative Example 3 that the addition of bisphenol A epoxy novolac copolymer significantly improves the polishing rate and wear resistance compared to the addition of common bisphenol A epoxy prepolymer.
[0217] It can be seen from the data of Example 5 and Comparative Example 4 that the corona treatment can increase the polishing rate stability of the polishing pad, so that the polishing rate of each round of polishing is not much different.
[0218] The polishing pads prepared in the embodiments mentioned in this patent all have better polishing rate and wear resistance than commercially available products.
[0219] It can be seen from Table 4 that:
[0220] It can be seen from Examples 5 to 6 and Comparative Examples 1 to 4 that corona treatment can increase the service life of the polishing pad. The polishing pads prepared in the examples of this patent have a significantly longer service life than commercially available products under different polishing liquid environments.
[0221] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.
Claims
1. A chemical oxidation resistant polishing pad, characterized in that: The invention comprises the following raw material components: polyurethane prepolymer, bisphenol A epoxy phenolic copolymer, chain extender and foaming agent.
2. The chemical oxidation resistant polishing pad according to claim 1, characterized in that: The raw material components include the following parts by weight: Polyurethane prepolymer 90-110 parts 2.5-15 parts of bisphenol A epoxy novolac copolymer Chain extender 30-70 parts Foaming agent 0.05~2 parts.
3. The chemical oxidation resistant polishing pad according to claim 1, characterized in that: The invention comprises one or more of the following features: the Shore hardness of the polyurethane prepolymer is 73-75HD; The content of isocyanate groups in the polyurethane prepolymer is 9.4-9.7wt%; The polyurethane prepolymer is prepared by reacting polyether polyol and toluene diisocyanate.
4. The chemical oxidation resistant polishing pad according to claim 1, characterized in that: The invention comprises one or more of the following features: the bisphenol A epoxy novolac copolymer is obtained by copolymerizing a bisphenol A type epoxy prepolymer and a phenolic condensation polymer; The chain extender is 3,5-diethyltoluenediamine and / or 3,3'-dichloro-4,4'-diphenylmethanediamine; The foaming agent is water; The raw material components also include polyether diols; The raw material components also include a catalyst, and the catalyst includes triethylenediamine; The raw material components also include a surfactant.
5. The chemical oxidation resistant polishing pad according to claim 4, characterized in that: The invention comprises one or more of the following features: the mass ratio of the bisphenol A epoxy prepolymer to the phenolic condensation polymer is (7-30):3; The phenolic condensation polymer is a linear phenolic condensation polymer; The bisphenol A epoxy prepolymer has an epoxy equivalent of 171-175 g / eq and a viscosity of 4000-6000 mPa·s at 25° C.; The phenolic polycondensate has a viscosity of 350-450 mPa·s at 25°C; The non-volatile matter content of the phenolic polycondensate at 135° C. is 70-80%; The copolymerization reaction adopts a curing accelerator; The reaction temperature of the copolymerization is 150-160°C; The polyether diol is polytetrahydrofuran ether diol; The polyether diol is used in an amount of 10 to 30 parts; The amount of the catalyst is 0.03 to 0.2 parts; The catalyst further comprises a diol, wherein the diol is selected from one or more of dipropylene glycol, butanediol and ethylene glycol; In the catalyst, the content of triethylenediamine is 30-35wt%; The amount of the surfactant is 1 to 5 parts; The surfactant is one or more selected from linear polysiloxane, polydimethylsiloxane and polysiloxane-oxyalkylene block copolymer.
6. A method for preparing a chemical oxidation resistant polishing pad according to any one of claims 1 to 5, characterized in that: The raw material components are uniformly mixed and pre-cured to obtain the chemical oxidation resistant polishing pad.
7. The preparation method according to claim 6, characterized in that: Before mixing, the polyurethane prepolymer, the bisphenol A epoxy novolac copolymer, and the polyether diol are preheated; and / or, before mixing, the chain extender is preheated.
8. The preparation method according to claim 6, characterized in that: The pre-curing temperature is 75-85° C.; and / or, a post-curing treatment is performed after the pre-curing.
9. The preparation method according to claim 8, characterized in that: The post-curing temperature is 95-105° C.; and / or, slicing, grinding, grooving, surface cleaning and corona treatment are performed after the post-curing treatment; preferably, the input voltage of the corona treatment is AC300-400V, the power is 2-70KW, and the electrode gap is 1-2mm.
10. Use of the chemical oxidation resistant polishing pad according to any one of claims 1 to 5 as a polishing pad for polishing a SiC substrate in chemical mechanical polishing.
Citation Information
Patent Citations
PU solidified epoxy phenolic resin as well as preparation method and application thereof
CN101987882A
Laminated polishing pad
CN103476546A
Hot-melt adhesive sheet for laminated polishing pad and adhesive-layer-bearing support layer for laminated polishing pad
CN103492124A
Abrasive articles
GB1399673A
Epoxypolyol resin composition
JP2004352866A