A high modulus, low stress relaxation, easy-to-process polyurethane and its preparation method and application

Through specific combinations of raw materials and preparation methods, a full-hard segment design is formed, which solves the processing difficulty and stress relaxation problems of invisible orthodontic materials, realizes the characteristics of high modulus, low stress relaxation and easy processing, and improves the dental orthodontics performance.

CN118930810BActive Publication Date: 2024-12-06SICHUAN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411403962.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-10-09
Publication Date
2024-12-06
Estimated Expiration
2044-10-09

AI Technical Summary

Technical Problem

Existing invisible correction materials have challenges in processing difficulty and stress relaxation speed, resulting in high hardness of the material but difficult processing and unstable stress, affecting the thickness and treatment effect of the correction device.

Method used

Using a combination of histamine-type chain extender, small molecule diol chain extender and crosslinker, a specific molar ratio and dosage range, combined with diisocyanate and polyol or polyamine as raw materials, a complete set is formed by a specific preparation method. Hard segment design of polyurethane, introduces dynamic bonds to reduce processing temperature and improve modulus and stress retention capabilities.

Benefits of technology

It significantly reduces the processing temperature of polyurethane, improves the modulus and stress retention ability, enhances the easy-to-processability and stability of the material, and is suitable as an invisible tooth orthodontic material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930810B_ABST
    Figure CN118930810B_ABST
Patent Text Reader

Abstract

The present invention provides a high modulus, low stress relaxation, easy-to-process polyurethane and its preparation method and application, belonging to the field of biomedical materials. The above-mentioned polyurethane is prepared from the following raw materials: histamine type chain extender, small molecule diol chain extender, diisocyanate, cross-linking agent; the molar ratio of cross-linking agent to histamine type chain extender is 1: (4~12), the molar ratio of diisocyanate to small molecule diol is (0.98~1.16): 1, and the mass fraction of cross-linking agent in the raw material is less than 1%. The processing temperature of the polyurethane of the present invention is significantly lower than that of the commercially available Isoplast‑2530 product, and the modulus and stress retention ability are significantly improved, which has the potential to be used as a material for invisible dental braces.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention provides a high modulus, low stress relaxation, easy-to-process polyurethane and a preparation method and application thereof, belonging to the field of biomedical materials. Background Art

[0002] Thermoplastic polyurethane is a very versatile material with unique advantages in the application of invisible correction, such as excellent mechanical properties, chemical resistance, corrosion resistance and excellent transmittance. At present, the world's leading invisible correction solution providers Invisalign and Angelalign both use copolymerized polyurethanes of MDI and HDO, such as Isoplast-2530, as the main material for making orthodontic appliances. Among them, the application of MDI provides the material with a rich rigid structure and hydrogen bonding effect, which not only gives it a higher hardness and modulus, but also reduces the mobility of the chain segments, thereby reducing stress relaxation. However, it is precisely because of the rich intermolecular interactions in the material structure, such as hydrogen bonds and π-π stacking, which require higher energy to unlock them, that the material processing becomes more difficult. How to improve the machinability of this type of high-hardness material is a difficulty that needs to be solved urgently.

[0003] On the other hand, in long-term clinical use, researchers have found that existing materials still have the problem of unsatisfactory stress relaxation speed. Patients need to wear braces for about 22 hours a day. However, the stress that can be released by some braces drops to 50% of the initial loading after 8 hours of loading, which makes it difficult to maintain stable stress when transmitting force signals to the periodontal membrane. Regulating the interaction between chains, such as further increasing the density of hydrogen bond donors and acceptors, increasing chemical cross-linking, etc., can limit the slippage between chains and reduce stress relaxation. At the same time, adding more rigid structures to the molecular chain can limit the mobility of the molecular chain and regulate its stress relaxation ability. However, the application of these solutions will further increase the processing difficulty of the material itself, which is not conducive to clinical application.

[0004] In addition, the braces use the resilience of polymer materials to provide correction force. For the same material, under the condition of the same deformation, the release of correction force will increase with the increase of thickness. However, if the braces are too thick, it will not only affect the aesthetics and wearing comfort, but may also interfere with the patient's bite and cause problems such as posterior tooth opening and closing. Therefore, under the premise of pursuing the same correction force, choosing a material with a larger modulus can effectively reduce the required thickness of the braces. This reduction in thickness can significantly reduce the pad effect during invisible correction, thereby improving the treatment effect and the patient's experience.

[0005] Therefore, there is an urgent need to develop a new material suitable for dental braces that has high modulus, low stress relaxation and easy processing properties. Summary of the invention

[0006] The present invention provides a polyurethane, which is prepared from the following raw materials: a histamine chain extender, a small molecule diol chain extender, a diisocyanate, and a crosslinking agent; the molar ratio of the crosslinking agent to the histamine chain extender is 1:(4-12), the molar ratio of the diisocyanate to the small molecule diol is (0.98-1.16):1, and the mass fraction of the crosslinking agent in the raw materials is less than 1%;

[0007] The histamine type chain extender is a compound represented by formula A or a derivative thereof:

[0008]

[0009] Formula A

[0010] wherein m is an integer of 1 to 9; the derivative is a compound obtained by replacing the hydrogen on any carbon atom of the compound represented by formula A with a C1 to C10 alkyl group;

[0011] The small molecule diol chain extender is HO(CH2) p OH, where p is an integer from 3 to 8;

[0012] The diisocyanate is an aromatic diisocyanate;

[0013] The cross-linking agent is a polyol or a polyamine.

[0014] Furthermore, the above-mentioned histamine type chain extender is:

[0015]

[0016] The small molecule diol chain extender is HO(CH2) p OH, where p is an integer from 4 to 6;

[0017] The diisocyanate is one or more of diphenylmethane diisocyanate, meta-xylylene diisocyanate, and toluene diisocyanate;

[0018] The cross-linking agent is a polyol.

[0019] Furthermore, the polyol is one or more of trihydroxymethylpropane, glycerol, pentaerythritol, triethanolamine, tripropanolamine, and diethanol monoisopropanolamine.

[0020] Furthermore, the above-mentioned histamine type chain extender is

[0021] , the small molecule diol chain extender is 1,6-hexanediol, the diisocyanate is diphenylmethane diisocyanate, and the cross-linking agent is trihydroxymethylpropane.

[0022] Furthermore, the molar ratio of the cross-linking agent to the histamine chain extender is 1:(6~12); the molar ratio of the diisocyanate to the small molecule diol is (1.10~1.16):1, and the mass fraction of the cross-linking agent in the raw material is 0.2%~0.4%.

[0023] Furthermore, the molar ratio of the cross-linking agent to the histamine-type chain extender is 1:(9-12); and the mass fraction of the cross-linking agent in the raw material is 0.3-0.4%.

[0024] Preferably, the molar ratio of the crosslinking agent to the histamine chain extender is 1:9, and the mass fraction of the crosslinking agent in the raw material is 0.3; or the molar ratio of the crosslinking agent to the histamine chain extender is 1:12, and the mass fraction of the crosslinking agent in the raw material is 0.4.

[0025] The present invention also provides a method for preparing the polyurethane, comprising the following steps:

[0026] (1) Add a crosslinking agent to a small molecule diol chain extender and mix them evenly at a temperature of 45-55°C under anhydrous conditions;

[0027] (2) Add diisocyanate, stir for 0.5-1.5 minutes, and then mature at 95-105°C for 5-7 hours.

[0028] Furthermore, the temperature in step (1) is 50°C;

[0029] The stirring speed in step (2) is 900-1200 rpm, the aging temperature is 100° C., and the time is 6 hours; and the catalyst is added at the same time as the diisocyanate is added.

[0030] Furthermore, the catalyst is organic bismuth, and the added amount is 0.005-0.05%wt of the total amount of raw materials.

[0031] The present invention also provides application of the polyurethane in preparing materials for dental orthodontic appliances.

[0032] Beneficial effects of the present invention: The polyurethane of the present invention adopts a full hard segment design, selects specific diisocyanate, chain extender and cross-linking agent as raw materials, and within a specific dosage range, gives the polyurethane the characteristics of high modulus, low stress relaxation and easy processing. The processing temperature is significantly lower than that of the commercially available Isoplast-2530 product, and the modulus and stress retention capabilities are significantly improved, and it has the potential to be used as a material for invisible dental braces.

[0033] The polyols described in the present invention refer to alcohols containing three or more hydroxyl groups; and the polyamines refer to amines containing three or more amino groups.

[0034] The C1~C10 alkyl group mentioned in the present invention refers to a straight chain or branched chain alkyl group having 1, 2, ..., 10 carbon atoms.

[0035] Obviously, according to the above contents of the present invention, in accordance with common technical knowledge and customary means in the art, without departing from the above basic technical ideas of the present invention, other various forms of modification, replacement or change may be made.

[0036] The above contents of the present invention are further described in detail below through specific implementation methods in the form of embodiments. However, this should not be understood as the scope of the above subject matter of the present invention being limited to the following examples. All technologies realized based on the above contents of the present invention belong to the scope of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 a is the total reflection infrared spectrum of the polyurethane of the present invention (wave number range 1877 cm-1~1416 cm-1); Figure 1 b is the total reflection infrared spectrum of the polyurethane of the present invention (wave number range 3600 cm-1~650 cm-1).

[0038] Figure 2 It is the infrared spectrum of the isocyanate absorption peak changing with temperature. DETAILED DESCRIPTION

[0039] Example 1. Preparation of polyurethane of the present invention

[0040] 1,6-Hexanediol (HDO) (29.31g) was melted into a clear and transparent liquid under vacuum conditions, and diphenylmethane diisocyanate (MDI) (68.49g) was melted for use. The crosslinking agent trimethylolpropane (0.2g) was vacuum dehydrated at 100℃ for 2 hours and then cooled to 55℃, and added to the mixture of molten HDO and histamine (2g). The mixture was kept at 50℃ and stirred evenly. MDI liquid and 0.005g of organic bismuth catalyst were added. Stir at 1000rpm for about 1min. When the mixture was slightly exothermic, it was poured into a PTFE dish and aged at 100℃ for 6h to obtain polyurethane MPU0.2-IM2.

[0041] Example 2: Preparation of polyurethane of the present invention

[0042] 1,6-Hexanediol (HDO) (28.27 g) was melted under vacuum to form a clear and transparent liquid, and diphenylmethane diisocyanate (MDI) (68.53 g) was melted for use. The crosslinking agent trimethylolpropane (0.3 g) was vacuum dehydrated at 100 ° C for 2 hours and then cooled to 55 ° C, and added to the mixture of molten HDO and histamine (2 g). The mixture was kept at 50 ° C and stirred evenly. MDI liquid and 0.005 g of organic bismuth catalyst were added. Stir at 800 rpm for about 1 min. When the mixture was slightly exothermic, it was poured into a PTFE dish and aged at 100 ° C for 6 hours to obtain polyurethane MPU0.3-IM2.

[0043] Example 3: Preparation of polyurethane of the present invention

[0044] 1,6-Hexanediol (HDO) (29.07 g) was melted under vacuum to form a clear and transparent liquid, and diphenylmethane diisocyanate (MDI) (68.53 g) was melted for use. The crosslinking agent trimethylolpropane (0.4 g) was vacuum dehydrated at 100 ° C for 2 hours and then cooled to 55 ° C, and added to the mixture of molten HDO and histamine (2 g). The mixture was kept at 50 ° C and stirred evenly. MDI liquid and 0.005 g of organic bismuth catalyst were added. Stir at 1200 rpm for about 1 min. When the mixture was slightly exothermic, it was poured into a PTFE dish and aged at 100 ° C for 6 hours to obtain polyurethane MPU0.4-IM2.

[0045] Example 4. Preparation of polyurethane of the present invention

[0046] 1,6-Hexanediol (HDO) (28.15 g) was melted under vacuum to form a clear and transparent liquid, and diphenylmethane diisocyanate (MDI) (68.55 g) was melted for later use. The crosslinking agent trimethylolpropane (0.3 g) was vacuum dehydrated at 100 ° C for 2 hours and then cooled to 55 ° C, and added to the mixture of molten HDO and histamine (3 g). The mixture was kept at 50 ° C and stirred evenly. MDI liquid and 0.003 g of organic bismuth catalyst were added. Stir at 900 rpm for about 1 minute. When the mixture was slightly exothermic, it was poured into a PTFE dish and aged at 100 ° C for 6 hours to obtain polyurethane MPU0.3-IM3.

[0047] Example 5. Preparation of polyurethane of the present invention

[0048] 1,6-Hexanediol (HDO) (28.03 g) was melted into a clear and transparent liquid under vacuum conditions, and diphenylmethane diisocyanate (MDI) (68.57 g) was melted for use. The crosslinking agent trimethylolpropane (0.4 g) was vacuum dehydrated at 100 ° C for 2 hours and then cooled to 55 ° C, and added to the mixture of molten HDO and histamine (3 g). The mixture temperature was kept at 50 ° C and stirred evenly. MDI liquid and 0.005 g of organic bismuth catalyst were added. Stir at 1100 rpm for about 1 minute. When the mixture was slightly exothermic, it was poured into a PTFE dish and aged at 100 ° C for 6 hours to obtain polyurethane MPU0.4-IM3.

[0049] Comparative Example 1

[0050] 1,6-Hexanediol (HDO) (31.52 g) was melted under vacuum to form a clear and transparent liquid, and diphenylmethane diisocyanate (MDI) (68.38 g) was melted for use. The crosslinking agent trimethylolpropane (0.1 g) was vacuum dehydrated at 100 ° C for 2 hours, cooled to 55 ° C, and added to the molten HDO. The mixture was kept at 50 ° C and stirred evenly. MDI liquid and 0.003 g of organic bismuth catalyst were added. Stir at 1200 rpm for about 1 minute. When the mixture was slightly exothermic, it was poured into a PTFE dish and aged at 100 ° C for 6 hours to obtain polyurethane MPU0.1 without histamine-type chain extender.

[0051] Comparative Example 2

[0052] 1,6-Hexanediol (HDO) (31.28 g) was melted under vacuum to form a clear and transparent liquid, and diphenylmethane diisocyanate (MDI) (68.42 g) was melted for use. The crosslinking agent trimethylolpropane (0.3 g) was vacuum dehydrated at 100 ° C for 2 hours and then cooled to 55 ° C, and added to the molten HDO. The mixture was kept at 50 ° C and stirred evenly. MDI liquid and 0.01 g of organic bismuth catalyst were added. Stir at 1000 rpm for about 1 minute. When the mixture was slightly exothermic, it was poured into a PTFE dish and aged at 100 ° C for 6 hours to obtain polyurethane MPU0.3 without histamine-type chain extender.

[0053] Comparative Example 3

[0054] 1,6-Hexanediol (HDO) (30.76 g) was melted under vacuum to form a clear and transparent liquid, and diphenylmethane diisocyanate (MDI) (68.44 g) was melted for use. The crosslinking agent trimethylolpropane (0.3 g) was vacuum dehydrated at 100 ° C for 2 hours and then cooled to 55 ° C, and added to the mixture of molten HDO and histamine (0.5 g). The mixture was kept at 50 ° C and stirred evenly. MDI liquid and 0.01 g of organic bismuth catalyst were added. Stir at 1000 rpm for about 1 minute. When the mixture was slightly exothermic, it was poured into a PTFE dish and aged at 100 ° C for 6 hours to obtain polyurethane MPU0.3-IM0.5.

[0055] Comparative Example 4

[0056] 1,6-Hexanediol (HDO) (25.01 g) was melted under vacuum to form a clear and transparent liquid, and diphenylmethane diisocyanate (MDI) (68.68 g) was melted for use. The crosslinking agent trimethylolpropane (0.3 g) was vacuum dehydrated at 100 ° C for 2 hours and then cooled to 55 ° C, and added to the mixture of molten HDO and histamine (6 g). The mixture was kept at 50 ° C and stirred evenly. MDI liquid and 0.005 g of organic bismuth catalyst were added. Stir at 900 rpm for about 1 min. When the mixture was slightly exothermic, it was poured into a PTFE dish and aged at 100 ° C for 6 hours to obtain polyurethane MPU0.3-IM6.

[0057] Comparative Example 5

[0058] 1,6-Hexanediol (HDO) (29.43 g) was melted under vacuum to form a clear and transparent liquid, and diphenylmethane diisocyanate (MDI) (68.46 g) was melted for use. The crosslinking agent trimethylolpropane (0.1 g) was vacuum dehydrated at 100 ° C for 2 hours and then cooled to 55 ° C, and added to the mixture of molten HDO and histamine (2 g). The mixture was kept at 50 ° C and stirred evenly. MDI liquid and 0.004 g of organic bismuth catalyst were added. Stir at 1100 rpm for about 1 minute. When the mixture was slightly exothermic, it was poured into a PTFE dish and aged at 100 ° C for 6 hours to obtain polyurethane MPU0.1-IM2.

[0059] Comparative Example 6

[0060] 1,6-Hexanediol (HDO) (19.99 g) was melted under vacuum to form a clear and transparent liquid, and diphenylmethane diisocyanate (MDI) (69.01 g) was melted for use. The crosslinking agent trimethylolpropane (1 g) was vacuum dehydrated at 100°C for 2 hours and then cooled to 55°C, and added to the mixture of molten HDO and histamine (10 g). The mixture was kept at 50°C and stirred evenly. MDI liquid and 0.005 g of organic bismuth catalyst were added. Stir at 1200 rpm for about 1 minute. When the mixture was slightly exothermic, it was poured into a PTFE dish and aged at 100°C for 6 hours to obtain polyurethane MPU1.0-IM10.

[0061] Comparative Example 7

[0062] 1,6-Hexanediol (HDO) (27.23 g) was melted under vacuum to form a clear and transparent liquid, and diphenylmethane diisocyanate (MDI) (69.47 g) was melted for use. The crosslinking agent trimethylolpropane (0.4 g) was vacuum dehydrated at 100°C for 2 hours and then cooled to 55°C, and added to the mixture of molten HDO and dimethylglyoxime (4 g). The mixture was kept at 50°C and stirred evenly. MDI liquid and 0.005 g of organic bismuth catalyst were added. Stir at 900 rpm for about 1 minute. When the mixture was slightly exothermic, it was poured into a PTFE dish and aged at 100°C for 6 hours to obtain polyurethane MPU0.4-OX4.

[0063] Comparative Example 8

[0064] 1,6-Hexanediol (HDO) (27.14 g) was melted under vacuum to form a clear and transparent liquid, and diphenylmethane diisocyanate (HMDI) (69.56 g) was melted for use. The crosslinking agent trimethylolpropane (0.3 g) was vacuum dehydrated at 100 °C for 2 hours and then cooled to 55 °C, and added to the mixture of molten HDO and histamine (3 g). The mixture was kept at 50 °C and stirred evenly. MDI liquid and 0.01 g of organic bismuth catalyst were added. Stir at 1000 rpm for about 3 min. When the mixture was slightly exothermic, it was poured into a PTFE dish and aged at 100 °C for 6 h to obtain polyurethane HPU0.3-IM3.

[0065] Comparative Example 9

[0066] 1,6-Hexanediol (HDO) (30.27 g) was melted under vacuum to form a clear and transparent liquid, and diphenylmethane diisocyanate (HMDI) (69.43 g) was melted for use. The crosslinking agent trimethylolpropane (0.3 g) was vacuum dehydrated at 100 °C for 2 hours, cooled to 55 °C, and added to the molten HDO. The mixture was kept at 50 °C and stirred evenly. MDI liquid and 0.01 g of organic bismuth catalyst were added. Stir at 1000 rpm for about 3 min. When the mixture was slightly exothermic, it was poured into a PTFE dish and aged at 100 °C for 6 h to obtain polyurethane HPU0.3.

[0067] Table 1 Raw material dosage of examples and comparative examples

[0068]

[0069] Experimental Example 1: Characterization of the structure and solubility of polyurethane

[0070] Structural characterization: Cut the matured hard polyurethane sheet into 1 cm × 1 cm small pieces and place them on the infrared total reflection accessory, press them tightly and test them. The reflective crystal used in the accessory is diamond. The test number is set to 32 times, and the test wave number range is 4000-650 cm -1 , with a resolution of 4 cm -1 .

[0071] The results are as follows Figure 1 As shown, taking the total reflection infrared spectra of some embodiments and comparative examples as examples, from high wavenumber to low wavenumber, they correspond to the stretching vibration peaks of NH (~3200~3400 cm -1 ), CH stretching vibration peaks on benzene ring and methylene (~2940 cm -1 and ~2850 cm -1 ); stretching vibration peak of carbonyl group in carbamate bond (~1690 to ~1740 cm -1 ); C=C stretching vibration peak in benzene ring (~1590 cm -1 ); the stretching vibration peaks of CN and NH in the carbamate bond (~1540 cm -1 ); the skeleton vibration peak of the benzene ring (~1414 cm -1 ); CO stretching vibration peak in carbamate bond (~1221 cm -1 ). The spectra of the polyurethane with the addition of imidazole dynamic bonds are almost the same, but after the introduction, the stretching vibration peak of the carbonyl group in the carbamate bond is at 1670 cm -1 The sharp peak at 1510 cm -1The characteristic absorption peak representing the imidazole ring appeared at 2260 cm-1, indicating that the imidazole chain extender has been successfully synthesized into polyurethane. At the same time, no peaks attributable to -NCO (~2260 cm-1) were found in all samples. -1 ), indicating that it has been completely reacted; the above experimental results prove that the polyurethane of the present invention is successfully synthesized.

[0072] Experimental Example 2: Dynamic bond exchange and processing performance characterization

[0073] Dynamic bond exchange: The polyurethane of Example 5 was prepared into a thin film of ~10 μm and placed on a transmission type variable temperature infrared accessory. The test number was set to 32 times and the test wave number range was 4000-650 cm -1 , with a resolution of 4 cm -1 The test temperature range is 80-130 °C, the heating rate is 5 °C / min, and a test is performed every 10 °C rise.

[0074] The results are as follows Figure 2 When the temperature increased from 80°C to 130°C, the transmission infrared in the NCO region showed that the FTIR spectrum peak at 2260 cm-1 belonging to the isocyanate group in the polyurethane containing imidazole dynamic bonds began to appear and increase significantly, and the allophanate bond dissociated, proving that the histamine-type chain extender can successfully introduce dynamic bonds that can dissociate at lower temperatures into the polyurethane structure, which is beneficial to reduce the processing temperature of the polyurethane.

[0075] Determination of the hot pressing temperature of polyurethane: After the synthesized polyurethane is crushed into particles, it is vacuum dried at 100 °C for 8 h and packaged in a ziplock bag while hot. The flat plate vulcanizer is heated to the set temperature. After the temperature stabilizes, the dried polyurethane is added to the mold and evenly distributed. The mold is sent to the flat plate vulcanizer and plasticized for 4 min. After the granules soften, the bubbles in the mold are discharged, and a pressure of 10 MPa is applied and maintained for 1 min to compact it. After the hot pressing is completed, it is transferred to the cold pressing, and it is also kept at a pressure of 10 MPa for 5 min to make it close to room temperature. After cooling, the formed sheet is taken out and placed at room temperature for 1-2 days before preparing the sample for use. The flat plate vulcanizer is set at 180, 183, 185, 188, 190, 193, 195, 198, 200, 203, 205, 208, 210, 213, 215, 218, 220, 223, 225, 228, 230, 233, 235, 238, 240 ° C to test each polyurethane in descending order until the polyurethane film is uniform, complete, transparent and without silver streaks; this temperature is considered to be the appropriate temperature for hot pressing.

[0076] The polyurethane hot pressing molding temperatures of various embodiments and comparative examples are shown in Table 2. It can be seen that the processing temperature of the polyurethane hot pressing molding under the specific raw material composition ratio of the present invention is significantly lower than that of the Isoplast2530 polyurethane material currently widely used in invisible correction, and the processability is improved.

[0077] Experimental Example 3: Mechanical Properties Characterization

[0078] According to the type 2 dumbbell specimen standard in GB / T 528, the test specimens were cut out from the pressed film and tested using a universal material testing machine. Tensile test conditions: the test environment temperature is 37 °C, the gauge length is 25 mm, the stretching rate is 50 mm / min, and the modulus is calculated using the part with a strain of 0.01%-1%. Stress relaxation test conditions: the test environment temperature is 37 °C, the gauge length is 15 mm, the stretching rate is 50 mm / min, the tensile strain is set to 0.2% (0.3 mm), the test time is 1h, and the sampling frequency is 10Hz.

[0079] The results are shown in Table 2. The stress relaxation phenomenon of the polyurethane of the present invention is suppressed for 1 hour. The retention rate is higher than 85%, which is higher than the Isoplast 2530 polyurethane material currently widely used in invisible correction. The other comparative examples with different dosage ratios of the same raw materials have either low modulus and retention rate or high hot pressing molding temperature. In addition, it can be seen from comparative example 7 that the histamine in the system is replaced with dimethylglyoxime, that is, the dynamic covalent bond of the present invention is replaced with dimethylglyoxime-carbamate dynamic covalent bond (refer to Zhang L, Liu Z, Wu X, et al.A Highly Efficient Self-Healing Elastomer with Unprecedented Mechanical Properties[J].Advanced Materials, 2019, 31(23): 1901402.1-1901402.8. DOI: 10.1002 / adma.201901402.) After adding the diisocyanate in the system, it is difficult to achieve excellent modulus and retention rate under the same raw material dosage; at the same time, it can be seen from comparative examples 8-9 that after replacing the diisocyanate in the system with an aliphatic diisocyanate, the modulus and retention rate of the obtained polyurethane are significantly lower, and it is even difficult to reach the level of commercially available Isoplast-2530. In addition, in the polyurethane system prepared by aliphatic diisocyanate, the introduction of dynamic covalent bonds can reduce the polyurethane hot pressing molding temperature, but the degree of reduction is lower than that of the polyurethane system of aromatic diisocyanate of the present invention, that is, the improvement effect on processing performance is insufficient. Therefore, only the polyurethane prepared under the specific raw material type and dosage of the present invention can achieve excellent technical effects of high modulus, low stress relaxation and easy processing performance.

[0080] Table 2 Mechanical properties and hot pressing molding temperature of polyurethane in Examples and Comparative Examples

[0081]

[0082] In summary, the present invention provides a polyurethane with a full hard segment design, which uses specific diisocyanates, chain extenders and cross-linking agents as raw materials, introduces dynamic bonds and appropriate cross-linking structures, and gives the polyurethane the characteristics of high modulus, low stress relaxation and easy processing within a specific dosage range. The processing temperature is significantly lower than that of the commercially available Isoplast-2530 product, and the modulus and stress retention capabilities are significantly improved, so it has the potential to be used as a material for invisible dental braces.

Claims

1. A polyurethane, characterized in that The invention is prepared from the following raw materials: a histamine chain extender, a small molecule diol chain extender, a diisocyanate, and a crosslinking agent; the molar ratio of the crosslinking agent to the histamine chain extender is 1:(4-12), the molar ratio of the diisocyanate to the small molecule diol is (0.98-1.16):1, and the mass fraction of the crosslinking agent in the raw materials is less than 1%; The histamine type chain extender is a compound represented by formula A or a derivative thereof: wherein m is an integer of 1 to 9; the derivative is a compound obtained by replacing the hydrogen on any carbon atom of the compound represented by formula A with a C1 to C10 alkyl group; The small molecule diol chain extender is HO(CH2) p OH, wherein p is an integer from 3 to 8; The diisocyanate is an aromatic diisocyanate; The cross-linking agent is a polyol or a polyamine.

2. The polyurethane according to claim 1, characterized in that The histamine type chain extender is: The small molecule diol chain extender is HO(CH2) p OH, wherein p is an integer from 4 to 6; The diisocyanate is one or more of diphenylmethane diisocyanate, meta-xylylene diisocyanate, and toluene diisocyanate; The cross-linking agent is a polyol.

3. The polyurethane according to claim 2, characterized in that The polyol is one or more of trihydroxymethylpropane, glycerol, pentaerythritol, triethanolamine, tripropanolamine, and diethanol monoisopropanolamine.

4. The polyurethane according to claim 3, characterized in that The histamine type chain extender is The small molecule diol chain extender is 1,6-hexanediol, the diisocyanate is diphenylmethane diisocyanate, and the crosslinking agent is trihydroxymethylpropane.

5. The polyurethane according to claim 1, characterized in that The molar ratio of the crosslinking agent to the histamine chain extender is 1:(6-12); the molar ratio of the diisocyanate to the small molecule diol is (1.10-1.16):1, and the mass fraction of the crosslinking agent in the raw material is 0.2%-0.4%.

6. The polyurethane according to claim 5, characterized in that The molar ratio of the cross-linking agent to the histamine type chain extender is 1:(9-12); the mass fraction of the cross-linking agent in the raw material is 0.3-0.4%.

7. The method for preparing the polyurethane according to any one of claims 1 to 6, characterized in that: The steps include: (1) adding a crosslinking agent to a small molecule diol chain extender and mixing them uniformly at a temperature of 45 to 55° C. under anhydrous conditions; (2) Add diisocyanate, stir for 0.5 to 1.5 minutes, and then mature at 95 to 105°C for 5 to 7 hours.

8. The preparation method according to claim 7, characterized in that: The temperature in step (1) is 50° C. The stirring speed in step (2) is 900-1200 rpm, the aging temperature is 100° C., and the time is 6 hours; and the catalyst is added at the same time as the diisocyanate is added.

9. The preparation method according to claim 8, characterized in that: The catalyst is organic bismuth, and the added amount is 0.005-0.05%wt of the total amount of raw materials.

10. Use of the polyurethane according to any one of claims 1 to 6 in the preparation of materials for dental braces.