High-moisturizing protein deposition prevention contact lens and preparation method thereof
By constructing antibacterial coatings and gradient water molecules on hydrogel contact lenses, the problems of dryness and adsorption of precipitated substances under long-term wear are solved, and high moisturizing and anti-protein deposition is achieved, which is suitable for long-term use. Wear and improve wear comfort.
Patent Information
- Application Number
- CN202411192605.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-12
AI Technical Summary
Existing hydrogel contact lenses are prone to dryness when worn for a long time and easily absorb precipitated substances in tears, making it difficult to meet the requirements of long-term wear of corneal contact lenses.
Using a contact lens design that includes a hydrogel matrix, an antibacterial first coating and a second coating of gradient water molecules, the Zn-CuO coating and a second coating of gradient water content are constructed through surface deposition technology to inhibit protein adhesion and Keep your eyes moist.
Effectively prevent protein adsorption, keep eyes moist, suitable for long-term wear, and improve user wearing experience.
Smart Images

Figure CN118930935A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of contact lenses, and in particular to a highly moisturizing and protein deposition-resistant contact lens and a preparation method thereof. Background Art
[0002] Hydrogel is a three-dimensional cross-linked polymer generated by a simple reaction of one or more monomers. It has good swelling and water retention properties and is widely used in the fields of medicine and bioengineering materials. In addition, hydrogel is not only soft, can maintain a certain shape, and can absorb a large amount of water, but also has certain properties of solids and liquids. It is the main raw material for contact lenses.
[0003] Contact lenses, also called contact lenses, are lenses that are worn on the cornea of the eye to correct vision or protect the eyes. Contact lenses can not only bring great improvements to patients with refractive errors such as myopia, hyperopia, and astigmatism, but also have the advantages of being beautiful and convenient compared to ordinary glasses.
[0004] However, current hydrogel contact lenses tend to feel dry after long-term wear and are prone to absorbing precipitates in tears, making it difficult to meet the requirements for long-term wear of corneal contact lenses. Summary of the invention
[0005] In view of the above problems, the present application is proposed to provide a highly moisturizing and protein deposition-resistant contact lens and a preparation method thereof that overcomes the above problems or at least partially solves the above problems, comprising:
[0006] A highly moisturizing and protein deposition-resistant contact lens, comprising a hydrogel matrix, a first coating and a second coating, wherein the first coating is deposited on the surface of the hydrogel matrix, and the second coating is coated on the peripheral arc of the hydrogel matrix on which the first coating is deposited;
[0007] The hydrogel matrix comprises the following raw materials in parts by weight: 40-50 parts of a first monomer, 10-15 parts of a comonomer, 1-15 parts of methacryloylethyl sulfobetaine, 0.1-0.6 parts of a RAFT chain transfer agent, 0.5-1 parts of a first initiator, 1-2 parts of a crosslinking agent and 20-30 parts of deionized water;
[0008] The first coating is an antibacterial coating;
[0009] The distribution of water molecules in the second coating layer changes in a gradient. The second coating layer comprises the following raw materials in parts by weight: 40-50 parts of a second monomer, 0.1-1 parts of a second initiator, 30-60 parts of a solvent, 1-3 parts of a chain transfer agent and 0.001-0.05 parts of an inhibitor.
[0010] Furthermore, the first coating is a Zn-CuO coating with a thickness of 20-40 nm; and the water content of the second coating is 38%-55%.
[0011] Furthermore, the first monomer is hydroxyethyl methacrylate, and the comonomer is N-vinyl pyrrolidone.
[0012] Furthermore, the first initiator is at least one of azobisisobutyronitrile, azobisisoheptanenitrile, benzoyl peroxide, tert-butyl benzoyl peroxide, and methyl ethyl ketone peroxide.
[0013] Further, the crosslinking agent includes at least one of ethylene glycol dimethacrylate, diethylene glycol dimethacrylate, triethylene glycol dimethacrylate, ethylene glycol diacrylate, diethylene glycol diacrylate, polyethylene glycol diacrylate, glycerol trimethacrylate, glycerol triacrylate, glycerol dimethacrylate and glycerol diacrylate.
[0014] Furthermore, the hydrogel matrix further comprises an ultraviolet absorber and / or a colorant, wherein the ultraviolet absorber is a benzotriazole type monomer, and the colorant is a blue coloring monomer.
[0015] Further, the second monomer includes at least one of 2-hydroxyethyl methacrylate, acrylic acid, carboxyl acrylate, hydroxy acrylate, methyl methacrylate, methyl methacrylate, N-vinylpyrrolidone, N-vinylcaprolactam, N-vinylglutarimide and vinylpyridine.
[0016] Furthermore, the second initiator is at least one of azobisisobutyronitrile, azobisisoheptanenitrile, benzoyl peroxide, tert-butyl benzoyl peroxide, and methyl ethyl ketone peroxide.
[0017] The present invention also provides a method for preparing the above-mentioned highly moisturizing and protein deposition-resistant contact lens, comprising:
[0018] The first monomer, the comonomer, the methacryloylethyl sulfobetaine, the RAFT chain transfer agent, the first initiator, the crosslinking agent and the deionized water are mixed according to a ratio, injected into a mold, and thermally initiated to react to obtain the hydrogel matrix;
[0019] Constructing the first coating on the surface of the hydrogel matrix by surface deposition technology;
[0020] The second coating is coated on the peripheral arc of the hydrogel matrix on which the first coating is deposited, and baking and hydration treatment are performed to obtain a target contact lens.
[0021] Furthermore, the step of mixing the first monomer, the comonomer, the methacryloylethyl sulfobetaine, the RAFT chain transfer agent, the first initiator, the crosslinking agent and the deionized water according to a ratio, injecting the mixture into a mold, and thermally initiating a reaction to obtain the hydrogel matrix comprises:
[0022] Mixing the sulfonate betaine monomer, the RAFT chain transfer agent and the deionized water, and adding the first initiator to obtain a sulfonate betaine polymer solution;
[0023] The sulfonate betaine polymer solution, the first monomer, the comonomer and the crosslinking agent are dispersed in the deionized water, and then the first initiator is added to initiate a thermal reaction to obtain the hydrogel matrix.
[0024] This application has the following advantages:
[0025] In the embodiments of the present application, in contrast to the problem in the prior art that "current hydrogel contact lenses are prone to dryness after long-term wear, are prone to adsorb precipitation substances in tears, and are difficult to meet the requirements of long-term wear of corneal contact lenses", the present application provides a highly moisturizing and anti-protein deposition solution, specifically comprising: a hydrogel matrix, a first coating and a second coating, wherein the first coating is deposited on the surface of the hydrogel matrix, and the second coating is applied to the peripheral arc of the hydrogel matrix on which the first coating is deposited; the hydrogel matrix comprises the following raw materials in parts by weight: 0-50 parts of the first monomer, 10-15 parts of the comonomer, 1-15 parts of methacryloylethyl sulfobetaine, 0.1-0.6 parts of the RAFT chain transfer agent, 0.5-1 parts of the first initiator, 1-2 parts of the crosslinking agent and 20-30 parts of deionized water; the first coating is an antibacterial coating; the distribution of water molecules in the second coating is a gradient change, and the second coating includes the following parts by weight of raw materials: 40-50 parts of the second monomer, 0.1-1 parts of the second initiator, 30-60 parts of the solvent, 1-3 parts of the chain transfer agent and 0.001-0.05 parts of the inhibitor. The present invention uses non-ionic materials to make the lens have a low adsorption capacity for protein. Water is the main carrier of oxygen transfer in contact lenses. The lens has a low water content and poor oxygen permeability, but the low water content lens has a small pore size and is not easy to adsorb precipitation substances in tears; the lens has a high water content and good oxygen permeability, but the high water content lens has a large pore size and is easy to adsorb precipitation substances in tears. The second coating can keep the eyes moist and is suitable for long-term wear; the hydrogel matrix prepared by sulfobetaine and the like can inhibit protein adhesion to the surface of the corneal contact lens, thereby improving the user's long-term wearing experience and avoiding eye discomfort. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] In order to more clearly illustrate the technical solution of the present application, the drawings required for use in the description of the present application will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0027] Figure 1 This is a schematic structural diagram of a highly moisturizing and protein deposition-resistant contact lens provided in one embodiment of the present application;
[0028] Figure 2 This is a flowchart of the steps of a method for preparing a highly moisturizing and protein deposition-resistant contact lens provided in one embodiment of the present application;
[0029] Figure 3 is a flowchart of the steps of S110 provided in an embodiment of the present application;
[0030] Figure 4 is a schematic diagram of the contact angle;
[0031] Figure 5 It is a graph showing the anti-protein adsorption performance of Examples 1-3. DETAILED DESCRIPTION
[0032] In order to make the objects, features and advantages of the present application more obvious and understandable, the present application is further described in detail below in conjunction with the accompanying drawings and specific implementation methods. Obviously, the described embodiments are part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in the field without creative work are within the scope of protection of the present application.
[0033] In one embodiment of the present application, refer to Figure 1 , providing a highly moisturizing and protein deposition-resistant contact lens, comprising a hydrogel matrix, a first coating and a second coating, wherein the first coating is deposited on the surface of the hydrogel matrix, and the second coating is coated on the peripheral arc of the hydrogel matrix on which the first coating is deposited;
[0034] The hydrogel matrix comprises the following raw materials in parts by weight: 40-50 parts of a first monomer, 10-15 parts of a comonomer, 1-15 parts of methacryloylethyl sulfobetaine, 0.1-0.6 parts of a RAFT chain transfer agent, 0.5-1 parts of a first initiator, 1-2 parts of a crosslinking agent and 20-30 parts of deionized water;
[0035] The first coating is an antibacterial coating;
[0036] The distribution of water molecules in the second coating layer changes in a gradient. The second coating layer comprises the following raw materials in parts by weight: 40-50 parts of a second monomer, 0.1-1 parts of a second initiator, 30-60 parts of a solvent, 1-3 parts of a chain transfer agent and 0.001-0.05 parts of an inhibitor.
[0037] In the embodiments of the present application, in contrast to the problem in the prior art that "current hydrogel contact lenses are prone to dryness after long-term wear, are prone to adsorb precipitation substances in tears, and are difficult to meet the requirements of long-term wear of corneal contact lenses", the present application provides a highly moisturizing and anti-protein deposition solution, specifically comprising: a hydrogel matrix, a first coating and a second coating, wherein the first coating is deposited on the surface of the hydrogel matrix, and the second coating is applied to the peripheral arc of the hydrogel matrix on which the first coating is deposited; the hydrogel matrix comprises the following raw materials in parts by weight: 0-50 parts of the first monomer, 10-15 parts of the comonomer, 1-15 parts of methacryloylethyl sulfobetaine, 0.1-0.6 parts of the RAFT chain transfer agent, 0.5-1 parts of the first initiator, 1-2 parts of the crosslinking agent and 20-30 parts of deionized water; the first coating is an antibacterial coating; the distribution of water molecules in the second coating is a gradient change, and the second coating includes the following parts by weight of raw materials: 40-50 parts of the second monomer, 0.1-1 parts of the second initiator, 30-60 parts of the solvent, 1-3 parts of the chain transfer agent and 0.001-0.05 parts of the inhibitor. The present invention uses non-ionic materials to make the lens have a low adsorption capacity for protein. Water is the main carrier of oxygen transfer in contact lenses. The lens has a low water content and poor oxygen permeability, but the low water content lens has a small pore size and is not easy to adsorb precipitation substances in tears; the lens has a high water content and good oxygen permeability, but the high water content lens has a large pore size and is easy to adsorb precipitation substances in tears. The second coating can keep the eyes moist and is suitable for long-term wear; the hydrogel matrix prepared by sulfobetaine and the like can inhibit protein adhesion to the surface of the corneal contact lens, thereby improving the user's long-term wearing experience and avoiding eye discomfort.
[0038] Next, a highly moisturizing and protein deposition-resistant contact lens in this exemplary embodiment will be further described.
[0039] It should be noted that the hydrogel matrix is prepared by active polymerization of the first monomer, the comonomer and the sulfobetaine monomer under the action of a RAFT agent. A first coating is constructed on the surface of the hydrogel matrix by using a surface deposition technique, and then a second coating having a gradient distribution of water molecules is applied to the peripheral arc of the hydrogel matrix.
[0040] As an example, the RAFT chain transfer agent is selected from one of benzyl dithiobenzoate, isobutyl dithiobenzoate, trithiocarbonate, 4-cyanodithiobenzoylvaleric acid or carboxymethylthiobenzoate.
[0041] In one embodiment of the present application, the first coating is a Zn-CuO coating with a thickness of 20-40 nm; the water content of the second coating is 38%-55%.
[0042] It should be noted that Zn-CuO is a composite nanoparticle and is a highly efficient inorganic antibacterial agent. Nanoparticles attach and penetrate bacteria through contact, thereby producing ROS in bacterial cells, enhancing lipid peroxidation reactions, and leading to cell death. Zn-CuO has good antibacterial ability against Pseudomonas aeruginosa and Streptococcus mutans. The second coating is polymerized into a second coating with a gradient water content by a second monomer, a second initiator, a solvent, a chain transfer agent, and an inhibitor. The second coating achieves an ideal humidity balance on the surface of the hydrogel lens by finely regulating the distribution of water content on its surface, significantly enhancing the wetting effect of the hydrogel surface, ensuring that the inner layer of the lens can retain enough moisture to fit and nourish the surface of the eyeball, while the outer layer prevents excessive volatilization of moisture, effectively inhibiting the loss of excess moisture.
[0043] In one embodiment of the present application, the first monomer is hydroxyethyl methacrylate, and the comonomer is N-vinyl pyrrolidone.
[0044] It should be noted that hydroxyethyl methacrylate (HEMA) is one of the basic monomers and has a hydroxyl group. Adding N-vinyl pyrrolidone ketone (NVP) to prepare non-ionic contact lenses can improve the softness, comfort and resistance to protein deposition of contact lens materials.
[0045] In one embodiment of the present application, the first initiator is at least one of azobisisobutyronitrile, azobisisoheptanenitrile, benzoyl peroxide, tert-butyl benzoyl peroxide, and methyl ethyl ketone peroxide.
[0046] As an example, the first initiator is a photoinitiator, which is used to initiate the polymerization reaction of the monomer. The first initiator is preferably azobisisoheptanenitrile (ADVN).
[0047] In one embodiment of the present application, the cross-linking agent includes at least one of ethylene glycol dimethacrylate, diethylene glycol dimethacrylate, triethylene glycol dimethacrylate, ethylene glycol diacrylate, diethylene glycol diacrylate, polyethylene glycol diacrylate, glycerol trimethacrylate, glycerol triacrylate, glycerol dimethacrylate and glycerol diacrylate.
[0048] As an example, the crosslinking agent generates chemical bonds between linear molecules, so that the linear molecules are connected to each other to form a network structure, thereby improving the crosslinking density and heat resistance of the polymer. The crosslinking agent is preferably ethylene glycol dimethacrylate (EGDMA).
[0049] In one embodiment of the present application, the hydrogel matrix further includes an ultraviolet absorber and / or a colorant, the ultraviolet absorber is a benzotriazole type monomer, and the colorant is a blue coloring monomer.
[0050] It should be noted that contact lenses can also add other functional monomers as needed, such as ultraviolet absorbers and colorants. Benzotriazol type has good ultraviolet absorption and antioxidant properties, which can protect the eyes from ultraviolet damage; colorants mainly give the lens color.
[0051] The second coating layer comprises the following raw materials in parts by weight: 40-50 parts of a second monomer, 0.1-1 parts of a second initiator, 30-60 parts of a solvent, 1-3 parts of a chain transfer agent, and 0.001-0.05 parts of a polymerization inhibitor. Specifically:
[0052] In one embodiment of the present application, the second monomer includes at least one of 2-hydroxyethyl methacrylate, acrylic acid, carboxyl acrylate, hydroxy acrylate, methyl methacrylate, methyl methacrylate, N-vinylpyrrolidone, N-vinylcaprolactam, N-vinylglutarimide and vinylpyridine.
[0053] In one embodiment of the present application, the second initiator is at least one of azobisisobutyronitrile, azobisisoheptanenitrile, benzoyl peroxide, tert-butyl benzoyl peroxide, and methyl ethyl ketone peroxide.
[0054] In one embodiment of the present application, the solvent includes at least one of tert-butyl alcohol, cyclopentanone and cyclohexanone.
[0055] In one embodiment of the present application, the chain transfer agent is 2-mercaptoethanol.
[0056] In one embodiment of the present application, the polymerization inhibitor includes at least one of methylhydroquinone, p-hydroxyanisole, pyrogallol, 2,5-di-tert-butylhydroquinone and sodium dimethyldithiocarbamate.
[0057] Reference Figure 2 and Figure 3 In one embodiment of the present application, there is also provided a method for preparing a highly moisturizing and protein deposition-resistant contact lens as described in any of the above embodiments, comprising the steps of:
[0058] S210, mixing the first monomer, the comonomer, the methacryloylethyl sulfobetaine, the RAFT chain transfer agent, the first initiator, the crosslinking agent and the deionized water according to a ratio, injecting the mixture into a mold, and subjecting the mixture to a thermal initiation reaction to obtain the hydrogel matrix.
[0059] S220, constructing the first coating on the surface of the hydrogel matrix by surface deposition technology;
[0060] S230, coating the second coating on the peripheral arc of the hydrogel matrix on which the first coating is deposited, and performing baking and hydration treatment to obtain a target contact lens.
[0061] As described in step S210, the first monomer, the comonomer, the methacryloylethyl sulfobetaine, the RAFT chain transfer agent, the first initiator, the crosslinking agent and the deionized water are mixed according to a ratio, injected into a mold, and thermally initiated to react to obtain the hydrogel matrix.
[0062] S2101, mixing the methacryloylethyl sulfonate betaine monomer, the RAFT chain transfer agent and the deionized water, and adding the first initiator to obtain a sulfonate betaine polymer solution;
[0063] S2102, dispersing the sulfonated betaine polymer solution, the first monomer, the comonomer and the cross-linking agent in the deionized water, adding the first initiator, and performing a thermal initiation reaction to obtain the hydrogel matrix.
[0064] As an example, the methacryloylethyl sulfobetaine, the RAFT chain transfer agent and the deionized water are mixed and stirred according to the ratio, and nitrogen is evacuated to keep the nitrogen protection, and then the first initiator is added to react, and then the first monomer, comonomer and cross-linking agent are added, and then injected into the mold to obtain the hydrogel matrix through thermal initiation reaction.
[0065] As described in step S220, the first coating is constructed on the surface of the hydrogel matrix by surface deposition technology.
[0066] As an example, a hydrogel contact lens is added to a Zn-CuO solution and subjected to ultrasonic chemical deposition for 20-40 minutes. After the deposition, the lens is cleaned with double deionized water (ddH2O).
[0067] As described in step S230, the second coating is coated on the peripheral arc of the hydrogel matrix on which the first coating is deposited, and baking and hydration treatment are performed to obtain a target contact lens.
[0068] As an example, the second monomer, the second initiator, the solvent and the chain transfer agent are mixed evenly according to the ratio, reacted at 60-80°C for 5-8 hours, and the inhibitor is added to stop the reaction to obtain a second coating. The second coating is applied to the peripheral arc of the hydrogel substrate deposited with the first coating, and baked in an oven. The baked contact lens is then hydrated to achieve swelling equilibrium of the hydrogel contact lens to obtain a target contact lens.
[0069] Example 1
[0070] Preparation of hydrogel matrix:
[0071] 9 parts of methyl methacryloylethyl sulfobetaine (SBMAⅡ), 0.2 parts of benzyl dithiobenzoate and 30 parts of deionized water were mixed and stirred, and nitrogen was passed through the vacuum to maintain nitrogen protection. Then 0.5 parts of azobisisobutyronitrile were added for reaction, and then 45 parts of hydroxyethyl methacrylate, 13 parts of N-vinyl pyrrolidone and 1 part of ethylene glycol dimethacrylate were added, and then injected into a mold for thermal initiation reaction to obtain a hydrogel matrix.
[0072] Example 2
[0073] Preparation of contact lenses to prevent protein deposition:
[0074] The hydrogel matrix prepared in Example 1 was added to a Zn-CuO solution and subjected to ultrasonic chemical deposition for 30 minutes. After the deposition, the lens was cleaned with double deionized water to obtain a protein deposition-resistant contact lens having a first coating.
[0075] Example 3
[0076] Preparation of highly moisturizing and anti-protein deposition contact lenses:
[0077] 32 parts of N-vinylpyrrolidone, 17 parts of 2-hydroxyethyl methacrylate, 0.1 parts of azobisisobutyronitrile, 42 parts of cyclopentanone, 16 parts of cyclohexanone and 1 part of 2-mercaptoethanol were mixed evenly, reacted at 70°C for 6 hours, 0.03 parts of inhibitor were added to stop the reaction, and a second coating was obtained. The second coating was applied to the peripheral arc of the contact lens of Example 2, and baked in an oven. The baked contact lens was then hydrated to achieve swelling equilibrium of the hydrogel contact lens, thereby obtaining a highly moisturizing and protein-resistant contact lens.
[0078] 1. Light transmittance test
[0079] Light transmittance is the percentage of light of a specific wavelength that passes through a material per unit thickness. When light passes through contact lenses, it will be refracted and reflected, which will interfere with the wearer's vision and cause a deviation between the world in the wearer's eyes and the real world. According to national standards, the light transmittance of soft hydrophilic contact lenses should not be less than 92%.
[0080] The optical fiber spectrometer was used to test the transmittance of the lenses of Examples 1 to 3. The test results are shown in Table 1 below. The transmittance of the contact lenses of Examples 1 to 3 at wavelengths of 400-800 nm was all above 92%.
[0081] 400nm 500nm 600nm 700nm 800nm Example 1 94.3 95.7 96.2 96.0 94.9 Example 2 93.6 94.2 95.1 94.6 93.8 Example 3 93.4 93.8 95.3 94.2 94.5
[0082] Table 1 Transmittance (%)
[0083] 2. Hydrophilicity test
[0084] The contact angle (θ) is a measure of the degree of wetting. Figure 4 As shown, θ refers to the angle between the tangent line of the solid-liquid contact edge and the solid plane when the liquid is dropped onto the solid surface. The contact angle can be used to measure the moisturizing performance of the care solution. The smaller the angle at which water stays on the surface, the more hydrophilic the surface is, the better the moisturizing performance is, and the more comfortable it is to wear. On the contrary, the larger the angle at which water stays on the solid surface, the more hydrophobic the surface is. The higher the hydrophilicity of the contact lens, the better the compatibility with the eyes, and the higher the wearing comfort. 90° is the dividing point between the hydrophilicity and hydrophobicity of the sample. The material is hydrophobic when it exceeds 90°, and hydrophilic when it is below 90°.
[0085] The contact angle of the material was measured by using a contact angle meter to analyze the sample. The contact lenses of Examples 1-3 were dried with filter paper and then laid flat on the surface of a glass carrier. Liquid was dripped onto the sample surface, and the moving image was taken and the contact angle data of the sample was obtained by digital image processing technology. Three groups of contact angle photos were collected and their average value was taken.
[0086] The surface wettability of Examples 1-3 is shown in Table 2. It can be seen that the contact angles of Examples 1-3 are all lower than 90°.
[0087] Example 1 Example 2 Example 3 Contact angle (°) 54.6 57.3 52.2
[0088] Table 2
[0089] 3. Anti-protein adsorption test
[0090] The contact lenses of Examples 1-3 were cut into 1×1 cm 2The blocks were soaked in 10 ml PBS solution for 30 min, then transferred to 10 ml 1.0 mg / ml bovine serum albumin solution and soaked for 24 h. 1 ml of the bovine serum albumin solution was taken, 5 ml of 0.1 mg / ml Coomassie Brilliant Blue solution was added and dyed for 5 min. The ultraviolet absorbance of the solution was measured at 595 nm, and the corresponding concentration of the solution after adsorption was calculated according to the standard curve.
[0091] The amount of protein adsorption was calculated as follows:
[0092]
[0093] In the formula, C 前 is the initial concentration of BSA; C 后 is the concentration of BSA after adsorption.
[0094] Reference Figure 5 , it can be seen that the anti-protein adsorption effects of Examples 1-3 increase successively.
[0095] Although the preferred embodiments of the present application have been described, those skilled in the art may make additional changes and modifications to these embodiments once they have learned the basic creative concept. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the embodiments of the present application.
[0096] Finally, it should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or terminal device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or terminal device. In the absence of further restrictions, the elements defined by the sentence "comprise a ..." do not exclude the existence of other identical elements in the process, method, article or terminal device including the elements.
[0097] The above is a detailed introduction to a highly moisturizing and protein deposition-proof contact lens, lens and preparation method thereof provided by the present application. Specific examples are used herein to illustrate the principle and implementation method of the present application. The description of the above embodiments is only used to help understand the method and core idea of the present application. At the same time, for a person skilled in the art, according to the idea of the present application, there may be changes in the specific implementation method and application scope. In summary, the content of this specification should not be understood as a limitation on the present application.
Claims
1. A highly moisturizing and protein deposition-resistant contact lens, characterized in that: It comprises a hydrogel matrix, a first coating and a second coating, wherein the first coating is deposited on the surface of the hydrogel matrix, and the second coating is coated on the peripheral arc of the hydrogel matrix on which the first coating is deposited; The hydrogel matrix comprises the following raw materials in parts by weight: 40-50 parts of a first monomer, 10-15 parts of a comonomer, 1-15 parts of methacryloylethyl sulfobetaine, 0.1-0.6 parts of a RAFT chain transfer agent, 0.5-1 parts of a first initiator, 1-2 parts of a crosslinking agent and 20-30 parts of deionized water; The first coating is an antibacterial coating; The distribution of water molecules in the second coating layer changes in a gradient. The second coating layer comprises the following raw materials in parts by weight: 40-50 parts of a second monomer, 0.1-1 parts of a second initiator, 30-60 parts of a solvent, 1-3 parts of a chain transfer agent and 0.001-0.05 parts of an inhibitor.
2. The highly moisturizing and protein deposition-resistant contact lens according to claim 1, characterized in that: The first coating is a Zn-CuO coating with a thickness of 20-40 nm; the water content of the second coating is 38%-55%.
3. The highly moisturizing and protein deposition-resistant contact lens according to claim 1, characterized in that: The first monomer is hydroxyethyl methacrylate, and the comonomer is N-vinyl pyrrolidone.
4. The highly moisturizing and protein deposition-resistant contact lens according to claim 1, characterized in that: The first initiator is at least one of azobisisobutyronitrile, azobisisoheptanenitrile, benzoyl peroxide, tert-butyl benzoyl peroxide, and methyl ethyl ketone peroxide.
5. The highly moisturizing and protein deposition-resistant contact lens according to claim 1, characterized in that: The crosslinking agent includes at least one of ethylene glycol dimethacrylate, diethylene glycol dimethacrylate, triethylene glycol dimethacrylate, ethylene glycol diacrylate, diethylene glycol diacrylate, polyethylene glycol diacrylate, glycerol trimethacrylate, glycerol triacrylate, glycerol dimethacrylate and glycerol diacrylate.
6. The highly moisturizing and protein deposition-resistant contact lens according to claim 1, characterized in that: The hydrogel matrix further comprises an ultraviolet absorber and / or a colorant, wherein the ultraviolet absorber is a benzotriazole type monomer and the colorant is a blue coloring monomer.
7. The highly moisturizing and protein deposition-resistant contact lens according to claim 1, characterized in that: The second monomer includes at least one of 2-hydroxyethyl methacrylate, acrylic acid, carboxyl acrylate, hydroxy acrylate, methyl methacrylate, methyl methacrylate, N-vinylpyrrolidone, N-vinylcaprolactam, N-vinylglutarimide and vinylpyridine.
8. The highly moisturizing and protein deposition-resistant contact lens according to claim 1, characterized in that: The second initiator is at least one of azobisisobutyronitrile, azobisisoheptanenitrile, benzoyl peroxide, tert-butyl benzoyl peroxide, and methyl ethyl ketone peroxide.
9. A method for preparing a highly moisturizing and protein deposition-resistant contact lens as claimed in claim 1, characterized in that: Includes steps: The first monomer, the comonomer, the methacryloylethyl sulfobetaine, the RAFT chain transfer agent, the first initiator, the crosslinking agent and the deionized water are mixed according to a ratio, injected into a mold, and thermally initiated to react to obtain the hydrogel matrix; Constructing the first coating on the surface of the hydrogel matrix by surface deposition technology; The second coating is coated on the peripheral arc of the hydrogel matrix on which the first coating is deposited, and baking and hydration treatment are performed to obtain a target contact lens.
10. The method for preparing highly moisturizing and protein deposition-resistant contact lenses according to claim 9, characterized in that: The step of mixing the first monomer, the comonomer, the methacryloylethyl sulfobetaine, the RAFT chain transfer agent, the first initiator, the crosslinking agent and the deionized water according to a ratio, injecting the mixture into a mold, and thermally initiating a reaction to obtain the hydrogel matrix comprises: Mixing the methacryloylethylsulfonate betaine monomer, the RAFT chain transfer agent and the deionized water, and adding the first initiator to obtain a sulfonate betaine polymer solution; The sulfonate betaine polymer solution, the first monomer, the comonomer and the crosslinking agent are dispersed in the deionized water, and then the first initiator is added to initiate a thermal reaction to obtain the hydrogel matrix.