Preparation method of antibacterial BOPA (biaxially-oriented polyamide) composite film capable of enhancing ink adhesion

The introduction of amino and guanidine groups through surface activation and modification treatment, and the zeolite imidazole ester skeleton material is applied to the surface of the BOPA film, which solves the problems of poor printing effect and low light transmittance of the BOPA film, and significantly improves the adhesion and barrier properties of the ink. Suitable for a wider range of packaging applications.

CN118930940APending Publication Date: 2024-11-12HESHAN YUNCHENG NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411073302.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The surface corona treatment effect of BOPA film deteriorates with the extension of storage time, affecting the printing firmness, and low light transmittance cannot effectively block light, limiting its application when packaging certain products that need to block light.

Method used

The amino and hydroxyl groups were introduced through surface activation treatment, the guanidine group was introduced through surface modification, and the zeolite imidazole ester skeleton structure material emulsion was coated on the surface of the film to construct a composite structure to improve ink adhesion and barrier properties.

Benefits of technology

It significantly enhances ink adhesion, reduces printing failures, extends shelf life, and improves gas and light barrier properties, expands the application range of BOPA films in the packaging field.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004981484330000071
    Figure BDA0004981484330000071
Patent Text Reader

Abstract

The invention relates to the technical field of preparation of BOPA (biaxially-oriented polyamide) films, and discloses a preparation method of an antibacterial BOPA composite film capable of enhancing ink adhesion, which comprises the following steps: treating a BOPA film subjected to low-temperature plasma treatment by using an alkaline aqueous solution, reacting by using a thiourea dioxide aqueous solution, coating by using a zeolite imidazate skeleton structure material emulsion and the like. The BOPA film with the surface containing amino and hydroxyl is further modified into a BOPA film with the surface containing guanidyl, and finally the BOPA composite film with the surface modified by guanidyl is formed. Through surface activation and surface modification, a composite structure is constructed on the BOPA film, guanidyl is introduced to improve the ink adhesion and antibacterial activity, and a zeolite imidazate skeleton structure material is added to improve the barrier property of the film. And through surface modification and composite structure construction, the light transmittance problem is further improved, so that the film is more suitable for various packaging and industrial applications.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of BOPA film preparation, and in particular relates to a method for preparing an antibacterial BOPA composite film capable of enhancing ink adhesion. Background Art

[0002] BOPA film is obtained by biaxially stretching nylon. It has excellent mechanical properties and barrier properties, so it is widely used in commodity packaging. However, although the molecular chain of BOPA film contains polar amide groups, it still needs to be corona treated before printing to improve the wettability and adhesion of the film to printing ink. This is because the surface corona treatment effect of BOPA film will gradually decline with the extension of storage time, thus affecting the firmness of subsequent printing.

[0003] In addition, BOPA film has a high light transmittance and cannot effectively block light, which limits the use of BOPA film in packaging certain products that need to block light.

[0004] In order to solve these problems, we proposed a method for preparing an antibacterial BOPA composite film that can enhance ink adhesion. By improving the structure of the BOPA film and adding a modification layer to improve its light transmittance and printing effect, its application range in the packaging field is expanded. Summary of the invention

[0005] In order to make up for the shortcomings of the existing technology, solve the problems of low light transmittance and poor printing effect of the existing BOPA film, and expand the application field of BOPA film in packaging, a method for preparing an antibacterial BOPA composite film that can enhance the adhesion of ink is proposed.

[0006] To achieve the above object, the present invention provides the following technical solutions:

[0007] A method for preparing an antibacterial BOPA composite film capable of enhancing ink adhesion comprises the following steps:

[0008] S1. Surface activation: soaking the BOPA film treated with low-temperature plasma in an alkaline aqueous solution, taking out the BOPA film after heating reaction, and washing it with deionized water until it is neutral, thereby obtaining a BOPA film containing amino groups and hydroxyl groups on the surface;

[0009] S2, surface modification: placing the surface activated BOPA film in a thiourea dioxide aqueous solution, heating for reaction, cooling, washing, and drying to obtain a guanidine-modified BOPA film;

[0010] S3, composite structure: coating the zeolite imidazolate skeleton structure material emulsion on the BOPA film with surface modified by guanidine groups, and drying by air blast; and then heating the composite polyethylene film to obtain the BOPA composite film with surface modified by guanidine groups.

[0011] Guanidine is a cationic group with strong protonation ability and antibacterial properties, and can generate electrostatic attraction with anionic groups in dyes. By using guanidine modifiers to react with amino groups on the surface of activated nylon film, BOPA film is modified with guanidine, which can effectively improve the adhesion of printed dyes, reduce printing failures, and give BOPA film antibacterial properties.

[0012] Zeolite imidazolate skeleton structure material is a nanomaterial with high porosity and large specific surface area, which has good gas adsorption and light-shielding properties. Applying the zeolite imidazolate skeleton structure material emulsion on the film surface can effectively block visible light and improve the gas barrier properties of the film.

[0013] Preferably, in step S1, the alkaline aqueous solution is one of an ammonia solution, a sodium carbonate solution, a sodium hydroxide solution, a potassium hydroxide solution, and a phosphate solution, and the pH of the alkaline aqueous solution is 8-10.

[0014] Preferably, in step S1, the alkaline aqueous solution is heated to 40-70° C. and reacted for 3-18 hours.

[0015] Preferably, in step S2, the thiourea dioxide aqueous solution is heated to 40-90° C. and reacted for 1-24 hours.

[0016] Preferably, in step S3, the temperature of the blast drying is 15-50°C.

[0017] Compared with the prior art, the technical effects and advantages of the present invention are:

[0018] BOPA film itself has good mechanical properties and barrier properties, but there are problems with light transmittance and poor printing effects. The present invention solves these problems by adding a modification layer on the surface of the BOPA film to improve its printing effect and application range. The main technologies include surface activation and surface modification, as well as the construction of a composite structure. Surface activation involves treating the BOPA film in an alkaline solution to introduce amino and hydroxyl groups. Surface modification introduces guanidine groups by reacting with thiourea dioxide to enhance ink adhesion and provide antibacterial properties. The composite structure improves the barrier properties of the film by adding zeolite imidazolate skeleton materials.

[0019] By introducing guanidine groups through surface modification, the adhesion between ink and BOPA film can be significantly enhanced, which can reduce failures during printing and improve printing quality. As a cationic group, guanidine groups have antibacterial properties, which can reduce bacterial contamination during printing and extend the shelf life of products. Adding zeolite imidazolate skeleton structure materials can effectively improve the gas barrier properties of the film and extend the shelf life of the items in the package.

[0020] BOPA film has good mechanical properties and barrier properties. Through surface modification and composite structure construction, its light transmittance problem is further improved, making it more suitable for a variety of packaging and industrial uses. The modifiers and additives used are environmentally friendly materials, which are in line with the current trend of green production and sustainable development. Since the composite film has good ink adhesion, antibacterial and barrier properties, it can be used in printing and packaging occasions that require higher barrier properties and longer durability. This preparation method improves the performance of BOPA film and can enhance the market competitiveness of the product without increasing too much cost. DETAILED DESCRIPTION

[0021] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0022] Example 1

[0023] The embodiment of the present application discloses a method for preparing an antibacterial BOPA composite film capable of enhancing ink adhesion. First, a BOPA film treated with low-temperature plasma is immersed in an alkaline aqueous solution with a pH of 8, heated to 40°C, reacted for 18 hours, the BOPA film is taken out, and washed with deionized water until neutral to obtain a BOPA film having amino groups and hydroxyls on the surface. Then, the BOPA film treated with surface activation is placed in a thiourea dioxide aqueous solution, heated to 40°C, reacted for 24 hours, cooled, washed, and dried to obtain a BOPA film with guanidine groups modified on the surface. Finally, a zeolite imidazolate skeleton structure material emulsion is coated on the BOPA film with guanidine groups modified on the surface, and air dried at room temperature; and then the composite polyethylene film is heated to obtain a BOPA composite film with guanidine groups modified on the surface.

[0024] Example 2

[0025] The embodiment of the present application discloses a method for preparing an antibacterial BOPA composite film that can enhance the adhesion of ink. First, a BOPA film treated with low-temperature plasma is immersed in an alkaline aqueous solution with a pH of 8, heated to 70°C, reacted for 3 hours, the BOPA film is taken out, and washed with deionized water until neutral to obtain a BOPA film containing amino groups and hydroxyls on the surface. Then, the BOPA film treated with surface activation is placed in a thiourea dioxide aqueous solution, heated to 90°C, reacted for 1 hour, cooled, washed, and dried to obtain a BOPA film with guanidine groups modified on the surface. Finally, a zeolite imidazolate skeleton structure material emulsion is coated on the BOPA film with guanidine groups modified on the surface, and air dried at room temperature; and then the composite polyethylene film is heated to obtain a BOPA composite film with guanidine groups modified on the surface.

[0026] Example 3

[0027] The embodiment of the present application discloses a method for preparing an antibacterial BOPA composite film that can enhance the adhesion of ink. First, a BOPA film treated with low-temperature plasma is immersed in an alkaline aqueous solution with a pH of 10, heated to 40°C, and reacted for 18 hours. The BOPA film is taken out and washed with deionized water until it is neutral to obtain a BOPA film having amino groups and hydroxyls on the surface. Then, the BOPA film treated with surface activation is placed in a thiourea dioxide aqueous solution, heated to 40°C, and reacted for 24 hours. After cooling, washing, and drying, a BOPA film with guanidine-modified surface is obtained. Finally, a zeolite imidazole ester skeleton structure material emulsion is coated on the BOPA film with guanidine-modified surface, and air-dried at room temperature; and then the composite polyethylene film is heated to obtain a BOPA composite film with guanidine-modified surface.

[0028] Example 4

[0029] The embodiment of the present application discloses a method for preparing an antibacterial BOPA composite film that can enhance the adhesion of ink. First, a BOPA film treated with low-temperature plasma is immersed in an alkaline aqueous solution with a pH of 10, heated to 70°C, and reacted for 3 hours. The BOPA film is taken out and washed with deionized water until it is neutral to obtain a BOPA film containing amino groups and hydroxyls on the surface. Then, the BOPA film treated with surface activation is placed in a thiourea dioxide aqueous solution, heated to 90°C, and reacted for 1 hour. After cooling, washing, and drying, a BOPA film with a surface modified with guanidine groups is obtained. Finally, a zeolite imidazole ester skeleton structure material emulsion is coated on the BOPA film with a surface modified with guanidine groups, and air drying is performed at room temperature. The composite polyethylene film is then heated to obtain a BOPA composite film with a surface modified with guanidine groups.

[0030] Example 5

[0031] The embodiment of the present application discloses a method for preparing an antibacterial BOPA composite film that can enhance the adhesion of ink. First, a BOPA film treated with low-temperature plasma is immersed in an alkaline aqueous solution with a pH of 9, heated to 50°C, and reacted for 15 hours. The BOPA film is taken out and washed with deionized water until it is neutral to obtain a BOPA film having amino groups and hydroxyls on the surface. Then, the BOPA film treated with surface activation is placed in a thiourea dioxide aqueous solution, heated to 50°C, and reacted for 20 hours. After cooling, washing, and drying, a BOPA film with a surface modified with guanidine groups is obtained. Finally, a zeolite imidazole ester skeleton structure material emulsion is coated on the BOPA film with a surface modified with guanidine groups, and air drying is performed at room temperature. The composite polyethylene film is then heated to obtain a BOPA composite film with a surface modified with guanidine groups.

[0032] Example 6

[0033] The embodiment of the present application discloses a method for preparing an antibacterial BOPA composite film that can enhance the adhesion of ink. First, a BOPA film treated with low-temperature plasma is immersed in an alkaline aqueous solution with a pH of 9, heated to 60°C, and reacted for 10 hours. The BOPA film is taken out and washed with deionized water until it is neutral to obtain a BOPA film having amino groups and hydroxyls on the surface. Then, the BOPA film treated with surface activation is placed in a thiourea dioxide aqueous solution, heated to 60°C, and reacted for 15 hours. After cooling, washing, and drying, a BOPA film with guanidine group-modified surface is obtained. Finally, a zeolite imidazole ester skeleton structure material emulsion is coated on the BOPA film with guanidine group-modified surface, and air-dried at room temperature. The composite polyethylene film is then heated to obtain a BOPA composite film with guanidine group-modified surface.

[0034] Example 7

[0035] The embodiment of the present application discloses a method for preparing an antibacterial BOPA composite film that can enhance the adhesion of ink. First, a BOPA film treated with low-temperature plasma is immersed in an alkaline aqueous solution with a pH of 9, heated to 60°C, and reacted for 5 hours. The BOPA film is taken out and washed with deionized water until it is neutral to obtain a BOPA film having amino groups and hydroxyls on the surface. Then, the BOPA film treated with surface activation is placed in a thiourea dioxide aqueous solution, heated to 70°C, and reacted for 10 hours. After cooling, washing, and drying, a BOPA film with a surface modified with guanidine groups is obtained. Finally, a zeolite imidazole ester skeleton structure material emulsion is coated on the BOPA film with a surface modified with guanidine groups, and air drying is performed at room temperature. The composite polyethylene film is then heated to obtain a BOPA composite film with a surface modified with guanidine groups.

[0036] Example 8

[0037] The embodiment of the present application discloses a method for preparing an antibacterial BOPA composite film that can enhance the adhesion of ink. First, a BOPA film treated with low-temperature plasma is immersed in an alkaline aqueous solution with a pH of 9, heated to 65°C, and reacted for 5 hours. The BOPA film is taken out and washed with deionized water until it is neutral to obtain a BOPA film having amino groups and hydroxyls on the surface. Then, the BOPA film treated with surface activation is placed in a thiourea dioxide aqueous solution, heated to 80°C, and reacted for 3 hours. After cooling, washing, and drying, a BOPA film with a surface modified with guanidine groups is obtained. Finally, a zeolite imidazole ester skeleton structure material emulsion is coated on the BOPA film with a surface modified with guanidine groups, and air drying is performed at room temperature. The composite polyethylene film is then heated to obtain a BOPA composite film with a surface modified with guanidine groups.

[0038] The room temperature during the forced air drying in Examples 1-8 is between 15 and 50°C.

[0039] The visible light blocking rate of the BOPA composite films prepared in Examples 1-8 was tested:

[0040] Cut a sample of appropriate size from the BOPA film, ensure that the surface of the sample is clean and uncontaminated, wipe it with alcohol if necessary, install the sample on the sample stage of the visible light rejection tester, turn on the test instrument, adjust the spectral range of 380 nanometers to 780 nanometers and the intensity of the standard light source of ISO 105-B1, start the test program, the instrument will automatically measure the intensity of light passing through the sample, record the test results, and calculate the rejection rate. See the performance test results table in Table 1. Analyze the visible light rejection performance of BOPA film based on the test results.

[0041] The oxygen permeability test was performed on the BOPA composite films prepared in Examples 1-8:

[0042] Cut a circular or rectangular sample from the BOPA film, ensure that the sample surface is clean and uncontaminated, place the sample in the sample chamber of the oxygen permeation test device, set the experimental conditions, such as temperature, humidity, etc., and adjust the air pressure difference, close the sample chamber, start to pass oxygen or air, measure the amount of oxygen passing through the sample per unit time, record the oxygen permeation data, calculate the oxygen permeability, see the performance test results table in Table 1, and analyze the oxygen barrier performance of the BOPA film based on the test results.

[0043] The BOPA composite films prepared in Examples 1-8 were tested for killing E. coli on the surface of the BOPA films:

[0044] Cut the sample from the BOPA film, make sure the surface of the sample is clean, wipe it with alcohol or other disinfectants when necessary, select a suitable sterilization method, such as ultraviolet irradiation, chemical disinfectant treatment, high temperature treatment, etc., set the appropriate sterilization time and temperature according to the selected method, evenly apply the E. coli suspension of known concentration on the surface of the film, ensure that the inoculation amount meets the experimental requirements to simulate the actual use conditions, place the inoculated sample under suitable temperature and humidity conditions for incubation, usually for 24 hours, to observe the sterilization effect, after incubation, observe whether E. coli grows on the surface of the sample, and count the colonies of the sample with E. coli growth, see the performance test results table in Table 1, and analyze the antibacterial properties of the BOPA film surface according to the results;

[0045]

[0046] The visible light blocking rate of the BOPA composite films of all examples reached more than 93%, among which Example 8 performed the best, reaching 98.5%. This shows that the surface-modified BOPA film has a better ability to block light, which helps to protect the products in the package from the influence of light.

[0047] The oxygen permeability of the embodiment is between 95.3 and 98.8 cm 3 / (㎡·24h·0.1MPa), indicating that the composite film has a good barrier effect on oxygen. The oxygen permeability of Example 8 is the lowest, indicating that this sample may have better gas barrier performance.

[0048] The sterilization amount of E. coli ranged from 71.6% to 80.5%, indicating that the surface-modified BOPA composite film had certain antibacterial properties. The sterilization amount of Example 8 was the highest, reaching 80.5%, indicating that the film not only provided good barrier properties, but also had strong antibacterial ability.

[0049] Based on the above results, it can be considered that the surface modification treatment significantly improves the performance of BOPA film, especially in terms of improving barrier properties and antibacterial properties. Example 8 performs best, which is attributed to its specific surface modification process, which makes the film have better barrier properties and antibacterial properties, making the composite film suitable for a wider range of packaging applications, especially in scenarios requiring higher barrier properties and hygienic properties.

[0050] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing an antibacterial BOPA composite film capable of enhancing ink adhesion, It is characterized in that The following steps are involved: S1. Surface activation: soaking the BOPA film treated with low-temperature plasma in an alkaline aqueous solution, taking out the BOPA film after heating reaction, and washing it with deionized water until it is neutral, thereby obtaining a BOPA film containing amino groups and hydroxyl groups on the surface; S2, surface modification: placing the surface activated BOPA film in a thiourea dioxide aqueous solution, heating for reaction, cooling, washing, and drying to obtain a guanidine-modified BOPA film; S3, composite structure: coating the zeolite imidazolate skeleton structure material emulsion on the BOPA film with surface modified by guanidine groups, and drying by air blast; and then heating the composite polyethylene film to obtain the BOPA composite film with surface modified by guanidine groups.

2. The method for preparing an antibacterial BOPA composite film capable of enhancing ink adhesion according to claim 1, Features: In step S1, the alkaline aqueous solution is one of an ammonia solution, a sodium carbonate solution, a sodium hydroxide solution, a potassium hydroxide solution, and a phosphate solution, and the pH of the alkaline aqueous solution is 8-10.

3. The method for preparing an antibacterial BOPA composite film capable of enhancing ink adhesion according to claim 1, Features: In step S1, the alkaline aqueous solution is heated to 40-70° C. and reacted for 3-18 hours.

4. The method for preparing an antibacterial BOPA composite film capable of enhancing ink adhesion according to claim 1, Features: In the step S2, the thiourea dioxide aqueous solution is heated to 40-90° C. and reacted for 1-24 hours.

5. The method for preparing an antibacterial BOPA composite film capable of enhancing ink adhesion according to claim 1, Features: In step S3, the temperature of the blast drying is 15-50°C.