Preparation method of full-biomass composite aerogel flame-retardant thermal insulation material
By introducing mica sheets and sodium lignin sulfonate into the gelatin matrix, using ice template induction method and vacuum freeze-drying technology to form a full biomass composite aerogel, solving the problems of flammability and fire hazards of biomass aerogels. Achieve high-performance flame retardant and environmentally friendly thermal insulation materials.
Patent Information
- Application Number
- CN202410834066.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-26
- Publication Date
- 2024-11-12
AI Technical Summary
Existing biomass aerogel insulation materials are flammable and dangerous to fire, and the introduction of inorganic nanomaterials or petroleum-based chemicals will damage their biodegradability, making it difficult to meet high-performance flame retardant and environmentally friendly requirements.
Ice template induction method and vacuum freeze-drying technology were used to introduce mica sheets and sodium lignin sulfonate into the gelatin matrix to form a full biomass composite aerogel, and mechanical and flame retardant properties were improved through the crosslinking network structure.
The prepared full biomass composite aerogel has excellent thermal stability, mechanical properties and flame retardant properties, is environmentally friendly, has low production costs, and is suitable for large-scale production.
Smart Images

Figure HDA0004912653500000011 
Figure HDA0004912653500000012 
Figure HDA0004912653500000013
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of composite aerogel preparation, and in particular to a method for preparing an all-biomass composite aerogel flame retardant and heat-insulating material. Background Art
[0002] Thermal insulation materials have long attracted human interest due to their ability to effectively manage thermal energy. In practical applications, these materials need to be tightly wrapped around the target surface to prevent heat exchange with the external environment. With the emergence of intelligent humans and industrial systems, new requirements have been put forward for the physical properties of these materials, and it is imperative to develop high-performance thermal insulation materials to meet these challenges. At present, thermal insulation materials can be divided into inorganic thermal insulation materials and organic thermal insulation materials according to their materials. However, organic thermal insulation materials, such as polyurethane and polystyrene, have problems such as environmental unfriendliness and poor fire resistance; inorganic materials mainly include rock wool, glass wool felt, etc., which have disadvantages such as poor thermal insulation effect and high density. Therefore, it is of great practical significance to design a lightweight, high-strength and environmentally friendly thermal insulation material.
[0003] In recent years, biomass-based all-biomass aerogel insulation materials are considered to be ideal green alternatives to traditional petroleum-based foam insulation materials due to their wide sources, environmental friendliness, biodegradability, light weight, and low thermal conductivity. However, their flammable and high fire hazard nature greatly limits their ultimate practical application. In order to improve the flame retardant properties of biomass aerogel insulation materials, recent research has focused on the use of inorganic nanocomposites and petroleum-based chemical hybridization strategies to construct complex synergistic network structures. However, the introduction of additional inorganic nanomaterials or petroleum-based chemicals often sacrifices some of the biodegradability of bio-based aerogels, which is contrary to the original intention of the green, safe, and degradable concept. Therefore, from the perspective of material sustainability, it is urgent to develop all-biomass renewable flame-retardant insulation aerogels.
[0004] As a material with special functions, gelatin has been widely used as an aerogel substrate in the field of thermal management in recent years due to its outstanding mechanical properties, rich surface hydrogen bonding interactions, wide applicable temperature range, and excellent radiation resistance. However, although gelatin has excellent charring ability, it is also a flammable polysaccharide material and needs to be enhanced by other means.
[0005] Lignin is the second largest natural polymer after cellulose. It is also a renewable resource with aromatic units as the main structural units. It has a wide source and huge output. Lignin has the characteristics of high carbon content and rigid structure, which can improve the mechanical strength and flame retardant properties of aerogels at the same time, and its polyhydroxyl groups can form a cross-linked network structure with gelatin, thereby further enhancing the mechanical properties of aerogels. Mica flakes are a two-dimensional layered inorganic mineral with a silicon-oxygen tetrahedron and aluminum-oxygen hexahedron crystal structure. It can block heat and smoke and improve the thermal oxidation resistance of aerogels. At present, there are few reports on the simultaneous use of lignin and mica flakes in flame-retardant gels, and a large part of lignin is directly discarded as waste. The high-value utilization of lignin is one of the effective ways to solve the above problems. Summary of the invention
[0006] The present invention aims to provide a method for preparing a full-biomass composite aerogel flame retardant and heat-insulating material. The present invention adopts an ice template induction method and a vacuum freeze-drying technology to prepare a full-biomass composite aerogel by introducing biomass mica sheets and sodium lignin sulfonate into a gelatin matrix. The present invention has a simple preparation process and low cost, and the prepared full-biomass composite aerogel has excellent thermal stability, mechanical and flame retardant properties.
[0007] The technical solution of the present invention is as follows:
[0008] A method for preparing a full-biomass composite aerogel flame retardant and heat-insulating material comprises the following steps:
[0009] (1) Dissolve gelatin in distilled water, then add mica powder and sodium lignin sulfonate (C 20 H 24 Na2O 10 S2), stirring and dispersing uniformly to obtain a mixed sol;
[0010] The mass ratio of gelatin, mica powder and sodium lignin sulfonate is 3-5:1-2:1-2;
[0011] Preferably, stirring at 60° C. and 500 r / min for 30 min allows the mica powder and sodium lignin sulfonate to be uniformly dispersed in the gelatin solution;
[0012] (2) placing the mixed sol obtained in step (1) in a mold, first standing it at room temperature to solidify into a jelly state, then freezing it in a directional freezing chamber filled with liquid nitrogen (-196° C.) until it is completely solidified, and then vacuum freeze-drying it to obtain the all-biomass composite aerogel flame retardant and thermal insulation material;
[0013] Preferably, the mixed sol is left to stand at room temperature for ≥6 hours to solidify the gelatin into a jelly-like state;
[0014] The preferred vacuum freeze drying temperature is -60°C and the time is 24 hours.
[0015] The technical principles of the present invention include:
[0016] The present invention first dissolves gelatin in deionized water, and then uniformly disperses mica flakes and sodium lignin sulfonate in the gelatin solution to obtain a mixed solution. A cross-linked network structure is formed through the interaction of hydroxyl groups and amino groups between sodium lignin sulfonate, mica flakes and gelatin. The mixed solution is placed in a mold and allowed to stand and solidify into a jelly state at room temperature. A three-dimensional porous structure is constructed using an ice template induction method, and water is sublimated using freeze-drying technology to form a composite aerogel with a high specific surface area, good mechanical properties and excellent thermal stability. The application of the ice template induction technology in the present invention can control the pore structure and morphology of the aerogel, and the production cost is very low. During the vacuum freeze-drying process, water is evaporated at low temperature without generating large heat and physical changes, thereby maintaining the structure and morphology of the original aerogel and avoiding the possibility of changes in the material structure.
[0017] In the traditional aerogel preparation process, chemical agents such as organic solvents are mostly used, which is difficult to avoid environmental pollution and has a negative impact on the production environment. All-biomass aerogels are environmentally friendly, and the production process is simple and the cost is relatively low. The reported biomass-based aerogels often have poor high temperature resistance and mechanical properties. Therefore, the current focus is to use a simple method to design and prepare all-biomass aerogels with high flame retardant mechanical properties. The gelatin used in the present invention can release nitrogen-containing inert gas during pyrolysis, which can dilute combustible gases and oxygen; the rigid aromatic ring unit and high carbon content of lignin can simultaneously improve the mechanical strength and flame retardant properties of the aerogel; mica sheets, as a two-dimensional layered silicate inorganic mineral, can play a role in blocking heat and smoke, and can improve the thermal oxidation resistance of the aerogel.
[0018] The beneficial effects of the present invention are:
[0019] 1. In the synthesis process of the present invention, sodium lignin sulfonate is used as a raw material. Through ion exchange reaction and chemical cross-linking, the mechanical stability of the aerogel can be improved. In addition, it has antioxidant properties and can effectively improve the flame retardant properties of the aerogel.
[0020] 2. In the synthesis process of the present invention, mica powder, an inorganic flame retardant, is used as a raw material. The flaky structure of the mica powder can form a barrier to resist the contact between the flame and the aerogel, slow down the transfer of heat and oxygen to the inside, and significantly improve the flame retardant properties of the aerogel.
[0021] 3. In the synthesis process of the present invention, the hydrogen bonding between sodium lignin sulfonate and mica powder leads to the formation of a uniform porous structure, which significantly improves the flame retardant properties of the aerogel and has greater application potential in the market.
[0022] 4. In the synthesis process, the present invention adopts the ice template induction method, which can effectively retain the microstructure and chemical stability, and adopts vacuum freeze-drying technology instead of traditional supercritical drying. In contrast, supercritical drying is more expensive and has higher catalytic properties to the sample, so it may cause some damage to its chemical stability and microstructure. Therefore, the vacuum freeze-drying method used in the present invention is more advantageous.
[0023] 5. In the synthesis process, the present invention uses all-biomass raw materials, which is more environmentally friendly and improves energy utilization. The preparation process is simple, safe, low-cost, and suitable for large-scale production. The prepared all-biomass-based composite aerogel has excellent high hardness, low density, thermal stability, mechanical and flame retardant properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 : SEM images of the all-biomass composite aerogels prepared in Examples 1 and 2.
[0025] Figure 2 : Stress-strain curves of the all-biomass composite aerogels prepared in Examples 1 and 2.
[0026] Figure 3 : Thermogravimetric curves of the all-biomass composite aerogels prepared in Examples 1 and 2.
[0027] Figure 4 : Curve of heat release rate (HRR) of all-biomass composite aerogel prepared in Examples 1 and 2 changing with time.
[0028] Figure 5 : Curve of the smoke release rate (SPR) of the all-biomass composite aerogel prepared in Examples 1 and 2 changing with time. DETAILED DESCRIPTION
[0029] The present invention is further described below by means of specific embodiments, but the protection scope of the present invention is not limited thereto.
[0030] Unless otherwise specified, the raw materials used in the examples can be obtained from commercial sources; the methods used are conventional methods unless otherwise specified.
[0031] In the following examples, bio-based mica powder: chemically pure, Guangzhou Bangyou Chemical Technology Co., Ltd.; sodium lignin sulfonate: analytically pure / 100 g, Hangzhou Shuangmu Chemical Co., Ltd.; biodegradable gelatin: chemically pure / 500 g, Sinopharm Chemical Reagent Co., Ltd.
[0032] Example 1
[0033] A method for preparing a composite block aerogel of all-biomass by incorporating bio-based mica powder and sodium lignin sulfonate into a biodegradable gelatin matrix comprises the following steps:
[0034] Take 3g of gelatin in a beaker, add 50ml of deionized water, and stir at 60℃ for 30min to make the gelatin particles completely dissolved in water. Then, add 1g of mica powder and 1g of sodium lignin sulfonate (C 20 H 24 Na2O 10 S2), and then stirred for 30 minutes. During this process, the mica powder and sodium lignin sulfonate were evenly dispersed in the gelatin solution. The resulting mixed sol was placed in a 10*10*1cm 3 The mold was placed in a directional freezing chamber filled with liquid nitrogen (-196°C) for 15 minutes. After it was completely solidified, it was placed in a vacuum drying oven for freeze drying for 24 hours and then taken out to obtain a gelatin matrix block composite aerogel.
[0035] The maximum heat release rate of the gelatin matrix composite aerogel prepared in this example is 64.716 W / g, and the compressive strength at 70% compression deformation is 2.221 MPa.
[0036] Figure 1 In FIG. 8 , b is a SEM image of the sodium lignin sulfonate-gelatin-mica sheet composite aerogel prepared in this example. It can be seen from the figure that the sodium lignin sulfonate-gelatin-mica sheet composite aerogel forms a uniform porous structure.
[0037] Figure 2 In the figure, Gel3M1LS1 is the stress-strain curve of the sodium lignin sulfonate-gelatin-mica sheet composite aerogel prepared in this example. It can be seen from the figure that the sodium lignin sulfonate-gelatin-mica sheet composite aerogel has good mechanical properties.
[0038] Figure 3 In the figure, Gel3M1LS1 is the thermogravimetric curve of the sodium lignin sulfonate-gelatin-mica sheet composite aerogel prepared in this embodiment. It can be seen from the figure that after adding sodium lignin sulfonate and mica sheets, the thermal decomposition weight loss curve of the aerogel in the carbonization stage of gelatin (600°C-800°C) tends to be gentle, and the proportion of weight loss is very small.
[0039] Figure 4 In the figure, Gel3M1LS1 is a curve showing the heat release rate (HRR) of the sodium lignin sulfonate-gelatin-mica sheet composite aerogel prepared in this example over time. It can be seen from the figure that the addition of mica powder and sodium lignin sulfonate effectively limits the heat release of gelatin aerogel.
[0040] Figure 5 In the figure, Gel3M1LS1 is a curve of the smoke release rate (SPR) of the sodium lignin sulfonate-gelatin-mica sheet composite aerogel prepared in this example changing with time. It can be seen from the figure that the introduction of mica powder and sodium lignin sulfonate leads to a decrease in THR and av-EHC values, reflecting a reduction in the amount of combustible gas generated.
[0041] Example 2
[0042] A method for preparing bulk aerogel from a biodegradable gelatin matrix comprises the steps of:
[0043] Take 5g of gelatin in a beaker, add 50ml of deionized water, and stir at 60℃ for 30min to make the gelatin particles completely dissolved in water. 3 The mold was placed in a directional freezing chamber filled with liquid nitrogen (-196°C) for 15 minutes. After it was completely solidified, it was placed in a vacuum drying oven for freeze drying for 24 hours and then taken out to obtain pure gelatin block aerogel.
[0044] The maximum heat release rate of the pure gelatin block aerogel prepared in this example is 149.9 W / g, and the compressive strength at 70% compression deformation is 2.678 MPa.
[0045] Figure 1 In the figure, a is the SEM image of the pure gelatin block aerogel prepared in this example. It can be seen from the figure that the pure gelatin block aerogel has a lamellar structure inside.
[0046] Figure 2 In the figure, Gel5 is the stress-strain curve of the pure gelatin block aerogel prepared in this embodiment. It can be seen from the figure that after adding sodium lignin sulfonate and mica flakes, the stress value of the aerogel decreases because the mica powder has the granular characteristics and is not mixed evenly with the gelatin solution.
[0047] Figure 3 In FIG. 5 , Gel5 is the thermogravimetric curve of the pure gelatin block aerogel prepared in this example. It can be seen from the figure that the thermal decomposition weight loss curve of the aerogel decreases sharply during the carbonization stage of gelatin at (600° C.-800° C.).
[0048] Figure 4 In the figure, Gel5 is a curve of the heat release rate (HRR) of the pure gelatin block aerogel prepared in this embodiment changing with time. It can be seen from the figure that the pure gelatin aerogel triggers combustion after being heated for 128 seconds, and its instantaneous heat release rate (HRR) rises sharply and reaches a peak value.
[0049] Figure 5In the figure, Gel5 is a curve showing the smoke release rate (SPR) of the pure gelatin block aerogel prepared in this example changing with time. It can be seen from the figure that the pure gelatin aerogel generates a larger amount of combustible gas.
[0050] Example 3
[0051] A method for preparing a composite block aerogel of all-biomass by incorporating bio-based mica powder and sodium lignin sulfonate into a biodegradable gelatin matrix comprises the following steps:
[0052] Take 4g of gelatin in a beaker, add 50ml of deionized water, and stir at 60℃ for 30min to make the gelatin particles completely dissolved in water. Then, add 1g of sodium lignin sulfonate (C 20 H 24 Na2O 10 S2), and then stirred for 30 min. During this process, sodium lignin sulfonate was evenly dispersed in the gelatin solution. The resulting mixed sol was placed in a 10*10*1 cm 3 The mold was placed in a directional freezing chamber filled with liquid nitrogen (-196°C) for 15 minutes. After it was completely solidified, it was placed in a vacuum drying oven for freeze drying for 24 hours and then taken out to obtain a gelatin matrix block composite aerogel.
[0053] The maximum heat release rate of the gelatin matrix composite aerogel prepared in this example is 120.033 W / g, and the compressive strength at 70% compression deformation is 3.017 MPa.
[0054] Example 4
[0055] A method for preparing a composite block aerogel of all-biomass by incorporating bio-based mica powder and sodium lignin sulfonate into a biodegradable gelatin matrix comprises the following steps:
[0056] Take 2g mica powder and 5g gelatin in a beaker, add 50ml deionized water, and stir at 60℃ for 30min to make the gelatin particles completely dissolved in water. In this process, the mica powder is evenly dispersed in the gelatin solution. Place the obtained mixed sol in a 10*10*1cm 3 The mold was placed in a mold and left to stand for 6 hours, and the gelatin solidified into a jelly-like state at room temperature. Next, the mold was placed in a directional freezing chamber filled with liquid nitrogen (-196°C) and frozen for 15 minutes. After it was completely solidified, it was placed in a vacuum drying oven and freeze-dried for 24 hours before being taken out to obtain a gelatin matrix block composite aerogel.
[0057] The maximum heat release rate of the gelatin matrix composite aerogel prepared in this example is 79.383 W / g, and the compressive strength at 70% compression deformation is 1.820 MPa.
[0058] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Without departing from the scope of the technical solution of the present invention, equivalent embodiments made with slight modifications and equivalent changes using the above technical contents still belong to the scope of the technical solution of the present invention and should be included in the protection scope of the present invention.
Claims
1. A method for preparing a full-biomass composite aerogel flame retardant and thermal insulation material, characterized in that: The steps include: (1) dissolving gelatin in distilled water, then adding mica powder and sodium lignin sulfonate, stirring and dispersing them uniformly to obtain a mixed sol; (2) placing the mixed sol obtained in step (1) in a mold, first standing it at room temperature to solidify into a jelly state, then placing it in a directional freezing chamber filled with liquid nitrogen to freeze it until it is completely solidified, and then vacuum freeze-drying it to obtain the all-biomass composite aerogel flame retardant and thermal insulation material.
2. The method for preparing the all-biomass composite aerogel flame retardant and thermal insulation material according to claim 1, characterized in that: In step (1), the mass ratio of gelatin, mica powder and sodium lignin sulfonate is 3-5:1-2:1-2.
3. The method for preparing the all-biomass composite aerogel flame retardant and thermal insulation material according to claim 1, characterized in that: In step (1), the mica powder and sodium lignin sulfonate are uniformly dispersed in the gelatin solution at 60° C. and 500 r / min for 30 min.
4. The method for preparing the all-biomass composite aerogel flame retardant and thermal insulation material according to claim 1, characterized in that: In step (2), the mixed sol is allowed to stand at room temperature for ≥6 hours to allow the gelatin to solidify into a jelly state.
5. The method for preparing the all-biomass composite aerogel flame retardant and thermal insulation material according to claim 1, characterized in that: In step (2), the vacuum freeze drying temperature is -60°C and the time is 24 hours.
Citation Information
Cited By
Biomass aerogel with moisture absorption and photo-thermal desorption functions and preparation method thereof
CN119331305A