Fireproof thermal insulation material for building and preparation method of fireproof thermal insulation material
By combining modified cellulose powder, modified calcium hydroxide and basalt powder, combined with silicone waterproofing agent and VAE emulsion type interface agent, fire-proof insulation materials for building with excellent fire resistance and good thermal insulation properties are prepared by combining materials such as modified cellulose powder, modified calcium hydroxide and basalt powder, and combined with silicone waterproofing agent and VAE emulsion type interface agent, fire-proof insulation materials for building with excellent fire resistance and good thermal insulation properties are prepared. , solves the shortcomings of existing materials in fire resistance, thermal insulation effect and durability, and achieves higher safety and environmental protection.
Patent Information
- Application Number
- CN202411174288.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing fire-proof insulation materials for building have shortcomings in fire resistance, insulation effect, construction difficulty, durability and environmental protection, which affect the safety, comfort and sustainable development of buildings.
Using the synergistic effect of modified cellulose powder and modified calcium hydroxide, combined with basalt powder, silicone waterproofing agent and VAE emulsion type interface agent, fire-resistant with excellent fire resistance and good thermal insulation performance are prepared through molding and heat treatment. Insulation material.
It improves the fire resistance limit and flame retardant performance of the material, enhances the insulation and heat insulation ability, improves the mechanical strength and wear resistance, ensures the waterproof and moisture-proof function and environmental protection of the material, and is suitable for a variety of construction fields.
Smart Images

Figure CN118930983A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of building materials, and specifically discloses a fireproof and heat-insulating material for building and a preparation method thereof. Background Art
[0002] With the acceleration of modern urbanization, the construction industry has increasingly higher requirements for building materials. Especially in terms of energy saving, environmental protection and safety, the performance of building materials directly affects the overall performance of the building and the comfort and safety of the residents. Among them, fireproof and thermal insulation materials are an important part of the building, and their performance is directly related to the fire safety and energy efficiency of the building.
[0003] In the existing construction market, there are many types of fireproof and thermal insulation materials, but most of them have defects to varying degrees. Although traditional thermal insulation materials such as mineral wool and glass wool have certain thermal insulation effects, their fireproof performance is poor. They are easy to burn and produce toxic gases at high temperatures, which seriously threatens the safety of buildings. Some inorganic thermal insulation materials such as rock wool boards and foamed ceramic insulation boards, although they have good fireproof performance, often have problems such as many joints, poor waterproofness, and short service life during the construction process, which affects their application effect in actual projects.
[0004] In addition, with the advancement of science and technology in recent years, some new fireproof and thermal insulation materials have emerged, such as aerogels and nano flame retardants. These materials have improved fireproof performance and thermal insulation effects, but due to high production costs and complex construction processes, they have not yet been widely used. In summary, existing fireproof and thermal insulation materials for buildings have certain shortcomings in terms of fireproof performance, thermal insulation effect, construction difficulty, durability and environmental protection. Therefore, it is particularly important to develop a new type of fireproof and thermal insulation material that has both excellent fireproof performance and good thermal insulation effect. This will not only help improve the safety and comfort of buildings, but also promote the sustainable development of the construction industry. Summary of the invention
[0005] In order to solve the above problems, the present invention discloses a fireproof and heat-insulating material for building and a preparation method thereof.
[0006] The technical solution of the present invention is as follows:
[0007] A fireproof and heat-insulating material for construction, made from the following raw materials in parts by weight:
[0008] 100 parts of modified cellulose powder
[0009] Basalt powder 20-40 parts
[0010]
[0011] The modified cellulose powder is prepared by the following steps:
[0012] 1) dissolving oxalic acid in methyl benzoate solvent and uniformly mixing to obtain an oxalic acid solution;
[0013] 2) adding the titanate modifier dropwise to the oxalic acid solution and stirring evenly to obtain a mixed solution; adding the mixed solution dropwise to the cellulose powder and the silane coupling agent, mixing, stirring and reacting at 60-80° C. for 30-60 minutes, and then drying to obtain a block;
[0014] 3) In a twin-screw extruder, the block is melt-extruded, dried, ground into powder, and passed through a 200-mesh sieve to obtain modified cellulose powder.
[0015] Furthermore, in the above-mentioned fireproof and heat-insulating material for construction, the titanate modifier in step 1) is tetrabutyl titanate.
[0016] Furthermore, in the above-mentioned fireproof and heat-insulating material for construction, the silane coupling agent in step 2) is vinyl tris(β-methoxyethoxy)silane.
[0017] Furthermore, in the above-mentioned fireproof and heat-insulating material for construction, the modified cellulose powder is prepared by the following steps:
[0018] 1) adding 1 part of oxalic acid to 3-6 parts of methyl benzoate solvent by weight, and mixing them evenly to obtain an oxalic acid solution;
[0019] 2) adding 0.1-0.2 parts of tetrabutyl titanate dropwise to the above oxalic acid solution and stirring evenly to obtain a mixed solution;
[0020] The mixed solution is evenly added dropwise to 20-30 parts of cellulose powder, and then 3-6 parts of vinyl tri(β-methoxyethoxy) silane are added, stirred at 60-80°C for 30-60 minutes, and then dried to obtain a block;
[0021] 3) In a twin-screw extruder, the block is melt-extruded, dried, ground into powder, and passed through a 200-mesh sieve to obtain modified cellulose powder.
[0022] Furthermore, in the above-mentioned fireproof and heat-insulating material for construction, in step 3), the twin-screw extruder has twelve heating zones and one die head zone, the feed port is located at 1D of the first section of the extruder, and the extrusion parameters are:
[0023] The first section 1D is 132°C to 138°C, the second section 2D is 142°C to 148°C, the third section 3D is 152°C to 156°C, the fourth section 4D is 155°C to 160°C, the fifth section 5D is 155°C to 160°C, the sixth section 6D is 170°C to 175°C, the seventh section 7D is 175°C to 180°C, the eighth section 8D is 170°C-175°C, the ninth section 9D is 155°C to 160°C, the tenth section 10D is 145°C to 150°C, the eleventh section 11D is 140°C to 145°C, the twelfth section 12D is 145°C to 155°C, and the die head area is 140°C to 145°C.
[0024] Furthermore, in the above-mentioned fireproof and heat-insulating material for construction, the calcium hydroxide is modified calcium hydroxide, which is prepared by the following modification steps:
[0025] S1. The additives and deionized water were adjusted to prepare a digestion mixture; the additives were hydroxypropyl methylcellulose and methacrylic acid, and ultrasonic treatment was performed during the mixing process;
[0026] S2. The calcium oxide and the digestion mixture enter the quicklime digestion machine for digestion reaction to obtain calcium hydroxide slurry;
[0027] S3. The calcium hydroxide slurry was aged in an aging barrel for 12 h under stirring, and the refined calcium hydroxide slurry was then pressed into a filter cake by a filter press;
[0028] S4. After the filter cake is preliminarily pulverized, it is dried, broken into powder, and passed through a 100-mesh sieve to obtain modified calcium hydroxide.
[0029] In the step S1, the mass ratio of the additive to the deionized water is 1:2500, and the mass ratio of the hydroxypropyl methylcellulose to the methacrylic acid is 1:6.
[0030] In step S2, the solid-to-liquid ratio of quicklime to the digestion mixture is 1:10 g / mL.
[0031] Furthermore, in the above-mentioned fireproof and heat-insulating material for construction, the binder is ethylene glycol diacetate.
[0032] Furthermore, in the above-mentioned fireproof and thermal insulation material for construction, the waterproofing agent is a silicone waterproofing agent, and the interface treatment agent is a VAE emulsion-type interface agent.
[0033] The present invention also discloses a method for preparing the fireproof and heat-insulating building material, which comprises the following steps:
[0034] a. Mixing materials: first, uniformly mix the modified cellulose powder, basalt powder, calcium hydroxide, binder, waterproofing agent and interface treatment agent according to the proportion;
[0035] b Compression molding: Place the mixed material in the mold and flatten it, then press it into shape. After demoulding, place the green body on the bottom frame to prepare for curing;
[0036] c curing, heat treating and curing the green body to obtain a fireproof and thermal insulation material for construction; the curing temperature is 180-200° C., and the curing time is 1-3 hours.
[0037] Compared with the prior art, the present invention has the following beneficial effects:
[0038] The invention discloses a fireproof and heat-insulating material for building and a preparation method thereof. The fireproof and heat-insulating material has excellent fireproof performance: the fire resistance limit and flame retardant performance of the material are improved through the synergistic effect of modified cellulose powder and modified calcium hydroxide, and the fire spread is effectively prevented. The material of the invention also has good thermal insulation performance: the combination of modified cellulose powder and other raw materials enables the material to have excellent thermal insulation capacity, which helps to reduce the energy consumption of buildings; the addition of inorganic fillers such as basalt powder enhances the mechanical strength, hardness and wear resistance of the material, and improves the stability and durability of the overall structure. The addition of organosilicon waterproofing agent enables the material to have good waterproof and moisture-proof functions, protects the building from moisture erosion, and prolongs the service life; the application of VAE emulsion type interface agent improves the compatibility and bonding force between the components, ensures that the internal structure of the material is tight and gapless, and improves the overall performance. In addition, the invention adopts non-toxic or low-toxic raw materials for preparation, meets environmental protection requirements, and is harmless to human body and environment. It is suitable for a variety of building fields, such as wall insulation, roof insulation, pipeline insulation, etc., and has a high market application value. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 Comparative test of compressive strength MPa of Examples 1-4 and Comparative Examples 1-2;
[0040] Figure 2 The heat insulation capacity (m 2 ·K / W) comparison test. DETAILED DESCRIPTION
[0041] A fireproof and heat-insulating material for construction, made from the following raw materials in parts by weight:
[0042]
[0043] The modified cellulose powder is prepared by the following steps:
[0044] 1) adding 1 part of oxalic acid to 3-6 parts of methyl benzoate solvent by weight, and mixing them evenly to obtain an oxalic acid solution;
[0045] 2) adding 0.1-0.2 parts of tetrabutyl titanate dropwise to the above oxalic acid solution and stirring evenly to obtain a mixed solution;
[0046] The mixed solution is evenly added dropwise to 20-30 parts of cellulose powder, and then 3-6 parts of vinyl tri(β-methoxyethoxy) silane are added, stirred at 60-80°C for 30-60 minutes, and then dried to obtain a block;
[0047] 3) in a twin-screw extruder, the block is melt-extruded, dried, ground into powder, and passed through a 200-mesh sieve to obtain modified cellulose powder;
[0048] In the step 3), the twin-screw extruder has twelve heating zones and one die zone, the feed port is located at 1D of the first section of the extruder, and the extrusion parameters are:
[0049] The first section 1D is 132°C to 138°C, the second section 2D is 142°C to 148°C, the third section 3D is 152°C to 156°C, the fourth section 4D is 155°C to 160°C, the fifth section 5D is 155°C to 160°C, the sixth section 6D is 170°C to 175°C, the seventh section 7D is 175°C to 180°C, the eighth section 8D is 170°C-175°C, the ninth section 9D is 155°C to 160°C, the tenth section 10D is 145°C to 150°C, the eleventh section 11D is 140°C to 145°C, the twelfth section 12D is 145°C to 155°C, and the die head area is 140°C to 145°C.
[0050] The binder is ethylene glycol diacetate;
[0051] The waterproofing agent is an organic silicon waterproofing agent, and the interface treating agent is a VAE emulsion type interface agent.
[0052] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0053] The cellulose was purchased from Jinan Yuanfang Chemical Co., Ltd. and was HPMC hydroxypropyl methylcellulose.
[0054] Basalt powder was purchased from Nanjing Liuhe District Liuguang Yicai Stone Factory. High-grade gray powder. Apparent density: 1600kg / m 3 .
[0055] The organosilicon waterproofing agent was purchased from Jinan Chenwang Chemical Technology Co., Ltd. Sodium methylsiliconate waterproofing agent.
[0056] VAE emulsion type interface agent was purchased from Anhui Longyang Environmental Protection Technology Co., Ltd. VAE emulsion 707H emulsion waterproof interface agent.
[0057] Example 1
[0058] A fireproof and heat-insulating material for construction, made from the following raw materials in parts by weight:
[0059]
[0060] The modified cellulose powder is prepared by the following steps:
[0061] 1) adding 1 part of oxalic acid to 3 parts of methyl benzoate solvent by weight, and mixing them evenly to obtain an oxalic acid solution;
[0062] 2) adding 0.1 part of tetrabutyl titanate dropwise to the above oxalic acid solution and stirring evenly to obtain a mixed solution;
[0063] The mixed solution was evenly added dropwise to 20 parts of cellulose powder, and then 3 parts of vinyl tri(β-methoxyethoxy) silane were added, stirred at 60°C for 30 minutes, and then dried to obtain a block;
[0064] 3) in a twin-screw extruder, the block is melt-extruded, dried, ground into powder, and passed through a 200-mesh sieve to obtain modified cellulose powder;
[0065] In the step 3), the twin-screw extruder has twelve heating zones and one die zone, the feed port is located at 1D of the first section of the extruder, and the extrusion parameters are:
[0066] The first section 1D is 132°C to 138°C, the second section 2D is 142°C to 148°C, the third section 3D is 152°C to 156°C, the fourth section 4D is 155°C to 160°C, the fifth section 5D is 155°C to 160°C, the sixth section 6D is 170°C to 175°C, the seventh section 7D is 175°C to 180°C, the eighth section 8D is 170°C-175°C, the ninth section 9D is 155°C to 160°C, the tenth section 10D is 145°C to 150°C, the eleventh section 11D is 140°C to 145°C, the twelfth section 12D is 145°C to 155°C, and the die head area is 140°C to 145°C.
[0067] The binder is ethylene glycol diacetate;
[0068] The waterproofing agent is an organic silicon waterproofing agent, and the interface treating agent is a VAE emulsion type interface agent.
[0069] The method for preparing the above-mentioned thermal insulation material comprises the following steps:
[0070] a. Mixing materials: first, uniformly mix the modified cellulose powder, basalt powder, calcium hydroxide, binder, waterproofing agent and interface treatment agent according to the proportion;
[0071] b Compression molding: Place the mixed material in the mold and flatten it, then press it into shape. After demoulding, place the green body on the bottom frame to prepare for curing;
[0072] c curing, heat treating and curing the green body to obtain fireproof and thermal insulation materials for construction; the curing temperature is 190° C. and the curing time is 2 h.
[0073] Example 2
[0074] A fireproof and heat-insulating material for construction, made from the following raw materials in parts by weight:
[0075]
[0076] The modified cellulose powder is prepared by the following steps:
[0077] 1) adding 1 part of oxalic acid to 4.5 parts of methyl benzoate solvent by weight, and mixing them evenly to obtain an oxalic acid solution;
[0078] 2) adding 0.15 parts of tetrabutyl titanate dropwise to the above oxalic acid solution and stirring evenly to obtain a mixed solution;
[0079] The mixed solution was evenly added dropwise to 25 parts of cellulose powder, and then 4.5 parts of vinyl tri(β-methoxyethoxy) silane were added, stirred at 70°C for 45 minutes, and then dried to obtain a block;
[0080] 3) in a twin-screw extruder, the block is melt-extruded, dried, ground into powder, and passed through a 200-mesh sieve to obtain modified cellulose powder;
[0081] In the step 3), the twin-screw extruder has twelve heating zones and one die zone, the feed port is located at 1D of the first section of the extruder, and the extrusion parameters are:
[0082] The first section 1D is 132°C to 138°C, the second section 2D is 142°C to 148°C, the third section 3D is 152°C to 156°C, the fourth section 4D is 155°C to 160°C, the fifth section 5D is 155°C to 160°C, the sixth section 6D is 170°C to 175°C, the seventh section 7D is 175°C to 180°C, the eighth section 8D is 170°C-175°C, the ninth section 9D is 155°C to 160°C, the tenth section 10D is 145°C to 150°C, the eleventh section 11D is 140°C to 145°C, the twelfth section 12D is 145°C to 155°C, and the die head area is 140°C to 145°C.
[0083] The binder is ethylene glycol diacetate;
[0084] The waterproofing agent is an organic silicon waterproofing agent, and the interface treating agent is a VAE emulsion type interface agent.
[0085] The method for preparing the above-mentioned thermal insulation material comprises the following steps:
[0086] a. Mixing materials: first, uniformly mix the modified cellulose powder, basalt powder, calcium hydroxide, binder, waterproofing agent and interface treatment agent according to the proportion;
[0087] b Compression molding: Place the mixed material in the mold and flatten it, then press it into shape. After demoulding, place the green body on the bottom frame to prepare for curing;
[0088] c curing, heat treating and curing the green body to obtain fireproof and thermal insulation materials for construction; the curing temperature is 190° C. and the curing time is 2 h.
[0089] Example 3
[0090] A fireproof and heat-insulating material for construction, made from the following raw materials in parts by weight:
[0091] 100 parts of modified cellulose powder
[0092] Basalt powder 40 parts
[0093] Calcium hydroxide 20 parts
[0094] 20 parts of adhesive
[0095] 4 parts waterproofing agent
[0096] 2 parts of interface treatment agent
[0097] The modified cellulose powder is prepared by the following steps:
[0098] 1) adding 1 part of oxalic acid to 6 parts of methyl benzoate solvent by weight, and mixing them evenly to obtain an oxalic acid solution;
[0099] 2) adding 0.2 parts of tetrabutyl titanate to the above oxalic acid solution and stirring evenly to obtain a mixed solution; adding the mixed solution evenly to 30 parts of cellulose powder, and then adding 6 parts of vinyl tri(β-methoxyethoxy) silane, stirring and reacting at 80° C. for 60 minutes, and then drying to obtain a block;
[0100] 3) in a twin-screw extruder, the block is melt-extruded, dried, ground into powder, and passed through a 200-mesh sieve to obtain modified cellulose powder;
[0101] In the step 3), the twin-screw extruder has twelve heating zones and one die zone, the feed port is located at 1D of the first section of the extruder, and the extrusion parameters are:
[0102] The first section 1D is 132°C to 138°C, the second section 2D is 142°C to 148°C, the third section 3D is 152°C to 156°C, the fourth section 4D is 155°C to 160°C, the fifth section 5D is 155°C to 160°C, the sixth section 6D is 170°C to 175°C, the seventh section 7D is 175°C to 180°C, the eighth section 8D is 170°C-175°C, the ninth section 9D is 155°C to 160°C, the tenth section 10D is 145°C to 150°C, the eleventh section 11D is 140°C to 145°C, the twelfth section 12D is 145°C to 155°C, and the die head area is 140°C to 145°C.
[0103] The binder is ethylene glycol diacetate;
[0104] The waterproofing agent is an organic silicon waterproofing agent, and the interface treating agent is a VAE emulsion type interface agent.
[0105] The method for preparing the above-mentioned thermal insulation material comprises the following steps:
[0106] a. Mixing materials: first, uniformly mix the modified cellulose powder, basalt powder, calcium hydroxide, binder, waterproofing agent and interface treatment agent according to the proportion;
[0107] b Compression molding: Place the mixed material in the mold and flatten it, then press it into shape. After demoulding, place the green body on the bottom frame to prepare for curing;
[0108] c curing, heat treating and curing the green body to obtain fireproof and thermal insulation materials for construction; the curing temperature is 190° C. and the curing time is 2 h.
[0109] Example 4
[0110] A fireproof and heat-insulating material for construction, made from the following raw materials in parts by weight:
[0111]
[0112]
[0113] The modified cellulose powder is prepared by the following steps:
[0114] 1) adding 1 part of oxalic acid to 4.5 parts of methyl benzoate solvent by weight, and mixing them evenly to obtain an oxalic acid solution;
[0115] 2) adding 0.15 parts of tetrabutyl titanate dropwise to the above oxalic acid solution and stirring evenly to obtain a mixed solution;
[0116] The mixed solution was evenly added dropwise to 25 parts of cellulose powder, and then 4.5 parts of vinyl tri(β-methoxyethoxy) silane were added, stirred at 70°C for 45 minutes, and then dried to obtain a block;
[0117] 3) in a twin-screw extruder, the block is melt-extruded, dried, ground into powder, and passed through a 200-mesh sieve to obtain modified cellulose powder;
[0118] In the step 3), the twin-screw extruder has twelve heating zones and one die zone, the feed port is located at 1D of the first section of the extruder, and the extrusion parameters are:
[0119] The first section 1D is 132°C to 138°C, the second section 2D is 142°C to 148°C, the third section 3D is 152°C to 156°C, the fourth section 4D is 155°C to 160°C, the fifth section 5D is 155°C to 160°C, the sixth section 6D is 170°C to 175°C, the seventh section 7D is 175°C to 180°C, the eighth section 8D is 170°C-175°C, the ninth section 9D is 155°C to 160°C, the tenth section 10D is 145°C to 150°C, the eleventh section 11D is 140°C to 145°C, the twelfth section 12D is 145°C to 155°C, and the die head area is 140°C to 145°C.
[0120] The binder is ethylene glycol diacetate;
[0121] The waterproofing agent is an organic silicon waterproofing agent, and the interface treating agent is a VAE emulsion type interface agent.
[0122] The calcium hydroxide is modified calcium hydroxide, which is prepared by the following modification steps:
[0123] S1. The additives and deionized water were adjusted to prepare a digestion mixture; the additives were hydroxypropyl methylcellulose and methacrylic acid, and ultrasonic treatment was performed during the mixing process;
[0124] S2. The calcium oxide and the digestion mixture enter the quicklime digestion machine for digestion reaction to obtain calcium hydroxide slurry;
[0125] S3. The calcium hydroxide slurry was aged in an aging barrel for 12 h under stirring, and the refined calcium hydroxide slurry was then pressed into a filter cake by a filter press;
[0126] S4. After the filter cake is preliminarily pulverized, it is dried, broken into powder, and passed through a 100-mesh sieve to obtain modified calcium hydroxide.
[0127] In the step S1, the mass ratio of the additive to the deionized water is 1:2500, and the mass ratio of the hydroxypropyl methylcellulose to the methacrylic acid is 1:6.
[0128] In step S2, the solid-to-liquid ratio of quicklime to the digestion mixture is 1:10 g / mL.
[0129] The method for preparing the above-mentioned thermal insulation material comprises the following steps:
[0130] a. Mixing materials: first, uniformly mix the modified cellulose powder, basalt powder, calcium hydroxide, binder, waterproofing agent and interface treatment agent according to the proportion;
[0131] b Compression molding: Place the mixed material in the mold and flatten it, then press it into shape. After demoulding, place the green body on the bottom frame to prepare for curing;
[0132] c curing, heat treating and curing the green body to obtain fireproof and thermal insulation materials for construction; the curing temperature is 190° C. and the curing time is 2 h.
[0133] Comparative Example 1
[0134] A fireproof and heat-insulating material for construction, made from the following raw materials in parts by weight:
[0135]
[0136] The binder is ethylene glycol diacetate;
[0137] The waterproofing agent is an organic silicon waterproofing agent, and the interface treating agent is a VAE emulsion type interface agent.
[0138] The method for preparing the above-mentioned thermal insulation material comprises the following steps:
[0139] a. Mix the materials, firstly mix the cellulose powder, basalt powder, calcium hydroxide, binder, waterproofing agent and interface treatment agent evenly according to the proportion;
[0140] b Compression molding: Place the mixed material in the mold and flatten it, then press it into shape. After demoulding, place the green body on the bottom frame to prepare for curing;
[0141] c curing, heat treating and curing the green body to obtain fireproof and thermal insulation materials for construction; the curing temperature is 190° C. and the curing time is 2 h.
[0142] In this comparative example, cellulose powder was used instead of modified cellulose powder, and the other contents were the same as those in Example 2.
[0143] Comparative Example 2
[0144] A fireproof and heat-insulating material for construction, made from the following raw materials in parts by weight:
[0145]
[0146] The modified cellulose powder is prepared by the following steps:
[0147] 1) adding 1 part of oxalic acid to 4.5 parts of methyl benzoate solvent by weight, and mixing them evenly to obtain an oxalic acid solution;
[0148] 2) adding 0.15 parts of tetrabutyl titanate dropwise to the above oxalic acid solution and stirring evenly to obtain a mixed solution;
[0149] The mixed solution was evenly added dropwise to 25 parts of cellulose powder, and then 4.5 parts of vinyl tri(β-methoxyethoxy) silane were added, stirred at 70°C for 45 minutes, and then dried to obtain a block;
[0150] 3) in a twin-screw extruder, the block is melt-extruded, dried, ground into powder, and passed through a 200-mesh sieve to obtain modified cellulose powder;
[0151] In the step 3), the twin-screw extruder has twelve heating zones and one die zone, the feed port is located at 1D of the first section of the extruder, and the extrusion parameters are:
[0152] The first section 1D is 132°C to 138°C, the second section 2D is 142°C to 148°C, the third section 3D is 152°C to 156°C, the fourth section 4D is 155°C to 160°C, the fifth section 5D is 155°C to 160°C, the sixth section 6D is 170°C to 175°C, the seventh section 7D is 175°C to 180°C, the eighth section 8D is 170°C-175°C, the ninth section 9D is 155°C to 160°C, the tenth section 10D is 145°C to 150°C, the eleventh section 11D is 140°C to 145°C, the twelfth section 12D is 145°C to 155°C, and the die head area is 140°C to 145°C.
[0153] The binder is ethylene glycol diacetate;
[0154] The waterproofing agent is an organic silicon waterproofing agent, and the interface treating agent is a VAE emulsion type interface agent.
[0155] The method for preparing the above-mentioned thermal insulation material comprises the following steps:
[0156] a. Mixing materials: first, uniformly mix the modified cellulose powder, calcium hydroxide, binder, waterproofing agent and interface treatment agent according to the proportion;
[0157] b Compression molding: Place the mixed material in the mold and flatten it, then press it into shape. After demoulding, place the green body on the bottom frame to prepare for curing;
[0158] c curing, heat treating and curing the green body to obtain fireproof and thermal insulation materials for construction; the curing temperature is 190° C. and the curing time is 2 h.
[0159] This comparative example does not contain basalt powder, and the rest is the same as Example 2.
[0160] Test Example 1
[0161] The compressive strength and combustion performance were used to test the compressive strength and combustion performance of Examples 1-4 and Comparative Examples 1-2. A 100×100×100mm sample was prepared according to GB / T5486-2008 "Test Methods for Inorganic Rigid Thermal Insulation Products" and the compressive strength test was performed. The flame retardant properties of the material were determined according to "Classification of Combustion Performance of Building Materials and Products" (GB8624-2012). The thermal resistance m was determined using the guarded hot plate method: the steady-state heat transfer properties of a 100mm thick thermal insulation material were measured according to the standard GB / T 10294-2008. 2 ·K / W. The results are shown in Table 1 and Figure 1 and Figure 2 .
[0162] Table 1
[0163] serial number Compressive strengthMpa Flame retardant properties <![CDATA[Thermal insulation ability (m 2 ·K / W)]]> Example 1 9.23 A 2.91 Example 2 9.41 A 2.95 Example 3 9.39 A 3.02 Example 4 9.44 A 3.28 Comparative Example 1 9.31 B1 2.43 Comparative Example 2 7.19 A 2.71
[0164] It can be seen from Examples 1-4 that the fireproof and heat-insulating material prepared by the present invention has good compressive strength, flame retardancy and heat insulation performance, and its heat insulation capacity is better than that of a 100mm thick ordinary rock wool composite board of 2.5m 2 ·K / W; From the comparison between Examples 2 and 4, the use of modified calcium hydroxide can improve the thermal insulation capacity of the material of the present invention by about 10% (compared with before modification); From the comparison between Example 2 and Comparative Example 1, the use of modified cellulose can improve the thermal insulation capacity of cellulose by about 15%; From the comparison between Example 2 and Comparative Example 2, the addition of basalt powder can increase the compressive strength by more than 25% and further enhance the thermal insulation capacity.
[0165] In summary, the present invention discloses a fireproof and heat-insulating material for construction and a preparation method thereof, wherein the fireproof and heat-insulating material has excellent fireproof performance: through the synergistic effect of modified cellulose powder and modified calcium hydroxide, the fire resistance limit and flame retardant performance of the material are improved, and the spread of fire is effectively prevented. The material of the present invention also has good thermal insulation performance: the combination of modified cellulose powder and other raw materials enables the material to have excellent thermal insulation capabilities, which helps to reduce the energy consumption of buildings; the addition of inorganic fillers such as basalt powder enhances the mechanical strength, hardness and wear resistance of the material, and improves the stability and durability of the overall structure. The addition of organosilicon waterproofing agent enables the material to have good waterproof and moisture-proof functions, protects the building from moisture erosion, and prolongs the service life; the application of VAE emulsion type interface agent improves the compatibility and bonding force between the components, ensures that the internal structure of the material is tight and gapless, and improves the overall performance. In addition, the present invention adopts non-toxic or low-toxic raw materials for preparation, meets environmental protection requirements, and is harmless to the human body and the environment. It is suitable for a variety of construction fields, such as wall insulation, roof insulation, pipeline insulation, etc., and has a high market application value.
[0166] The above are limited to several preferred embodiments of the present invention, and the description is relatively specific and detailed, but it cannot be understood as limiting the scope of the present invention. It should be pointed out that for ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention.
Claims
1. A fireproof and heat-insulating material for construction, It is characterized in that Made from the following raw materials in parts by weight: The modified cellulose powder is prepared by the following steps: 1) dissolving oxalic acid in methyl benzoate solvent and uniformly mixing to obtain an oxalic acid solution; 2) adding the titanate modifier dropwise to the oxalic acid solution and stirring evenly to obtain a mixed solution; adding the mixed solution dropwise to the cellulose powder and the silane coupling agent, mixing, stirring and reacting at 60-80° C. for 30-60 minutes, and then drying to obtain a block; 3) In a twin-screw extruder, the block is melt-extruded, dried, ground into powder, and passed through a 200-mesh sieve to obtain modified cellulose powder.
2. A fireproof and heat-insulating material for construction according to claim 1, It is characterized in that The titanate modifier in step 1) is tetrabutyl titanate.
3. A fireproof and heat-insulating material for construction according to claim 1, It is characterized in that The silane coupling agent in step 2) is vinyl tris(β-methoxyethoxy)silane.
4. A fireproof and heat-insulating material for construction according to claim 1, It is characterized in that The modified cellulose powder is prepared by the following steps: 1) adding 1 part of oxalic acid to 3-6 parts of methyl benzoate solvent by weight, and mixing them evenly to obtain an oxalic acid solution; 2) adding 0.1-0.2 parts of tetrabutyl titanate dropwise to the above oxalic acid solution and stirring evenly to obtain a mixed solution; The mixed solution is evenly added dropwise to 20-30 parts of cellulose powder, and then 3-6 parts of vinyl tri(β-methoxyethoxy) silane are added, stirred at 60-80°C for 30-60 minutes, and then dried to obtain a block; 3) In a twin-screw extruder, the block is melt-extruded, dried, ground into powder, and passed through a 200-mesh sieve to obtain modified cellulose powder.
5. A fireproof and heat-insulating material for construction according to claim 4, It is characterized in that In the step 3), the twin-screw extruder has twelve heating zones and one die zone, the feed port is located at 1D of the first section of the extruder, and the extrusion parameters are: The first section 1D is 132°C to 138°C, the second section 2D is 142°C to 148°C, the third section 3D is 152°C to 156°C, the fourth section 4D is 155°C to 160°C, the fifth section 5D is 155°C to 160°C, the sixth section 6D is 170°C to 175°C, the seventh section 7D is 175°C to 180°C, the eighth section 8D is 170°C-175°C, the ninth section 9D is 155°C to 160°C, the tenth section 10D is 145°C to 150°C, the eleventh section 11D is 140°C to 145°C, the twelfth section 12D is 145°C to 155°C, and the die head area is 140°C to 145°C.
6. A fireproof and heat-insulating material for construction according to claim 1, It is characterized in that The calcium hydroxide is modified calcium hydroxide, which is prepared by the following modification steps: S1. The additives and deionized water were adjusted to prepare a digestion mixture; the additives were hydroxypropyl methylcellulose and methacrylic acid, and ultrasonic treatment was performed during the mixing process; S2. The calcium oxide and the digestion mixture enter the quicklime digestion machine for digestion reaction to obtain calcium hydroxide slurry; S3. The calcium hydroxide slurry was aged in an aging barrel for 12 h under stirring, and the refined calcium hydroxide slurry was then pressed into a filter cake by a filter press; S4. After the filter cake is preliminarily pulverized, it is dried, broken into powder, and passed through a 100-mesh sieve to obtain modified calcium hydroxide. In the step S1, the mass ratio of the additive to the deionized water is 1:2500, and the mass ratio of the hydroxypropyl methylcellulose to the methacrylic acid is 1:
6. In step S2, the solid-to-liquid ratio of quicklime to the digestion mixture is 1:10 g / mL.
7. A fireproof and heat-insulating material for construction according to claim 1, It is characterized in that The binder is ethylene glycol diacetate.
8. A fireproof and heat-insulating material for construction according to claim 1, It is characterized in that The waterproofing agent is an organic silicon waterproofing agent, and the interface treating agent is a VAE emulsion type interface agent.
9. A method for preparing a fireproof and heat-insulating building material according to any one of claims 1 to 8, It is characterized in that The following steps are involved: a. Mixing materials: first, uniformly mix the modified cellulose powder, basalt powder, calcium hydroxide, binder, waterproofing agent and interface treatment agent according to the proportion; b Compression molding: Place the mixed material in the mold and flatten it, then press it into shape. After demoulding, place the green body on the bottom frame to prepare for curing; c curing, heat treating and curing the green body to obtain a fireproof and thermal insulation material for construction; the curing temperature is 180-200° C., and the curing time is 1-3 hours.
10. Use of the fireproof and heat-insulating material according to any one of claims 1 to 8 in the preparation of heat insulation panels.
Citation Information
Patent Citations
Biomass fiber wall die block and preparation technology therefor
CN103420644A
Basalt long-fibre-reinforced wood-plastic sectional material and preparation method thereof
CN104073012A
Basalt composite fireproof new material and preparation method thereof
CN110304893A
Preparation method of high-activity and high-dispersion calcium hydroxide
CN117902839A
Insulation panel structure for construction
KR101954062B1