Wireless energy transmission high-frequency cable sheath material as well as preparation method and application thereof
By constructing an organic-inorganic hybrid network using a composite material composed of ethylene-vinyl acetate copolymer and ionic flame-retardant crosslinking sensitizer, the problems of insufficient conductivity, flame retardancy, and mechanical properties of high-frequency cable sheathing materials for wireless power transmission in subsonic vacuum pipeline flying cars are solved, and the material can be stably operated under high temperature and high stress environments.
Patent Information
- Application Number
- CN202411115745.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-12
AI Technical Summary
Existing technologies cannot provide high-conductivity, bend-resistant, stress-relaxation-resistant, and flame-retardant wireless power transmission high-frequency cable sheath materials suitable for subsonic vacuum tube flying cars, and cannot meet their long-term stable operation requirements under high temperature, high stress, and strong torsion environments.
A composite material composed of ethylene-vinyl acetate copolymer, rubber, ionic flame retardant crosslinking sensitizer, conductive filler, inorganic smoke-suppressing flame retardant, and phosphorus-based flame retardant is constructed through stepwise blending and electron beam irradiation crosslinking technology to build an organic-inorganic hybrid network structure, thereby improving the material's conductivity, flame retardancy, and mechanical properties.
The material has achieved long-term stable operation under high temperature, high stress and strong torsion environment, and its electrical conductivity, flame retardancy and mechanical properties have been improved, meeting the requirements of subsonic vacuum tube flying car.
Smart Images

Figure BDA0004993568370000021 
Figure BDA0004993568370000051 
Figure BDA0004993568370000052
Abstract
Description
Technical Field
[0001] The present invention relates to the field of polymer material technology and science, and in particular to a high-conductivity, bending-resistant, stress-relaxation-resistant, flame-retardant wireless energy transmission high-frequency cable sheath material for subsonic vacuum pipeline flying cars, and a preparation method and application thereof. Background Art
[0002] The subsonic vacuum tube train is a modern high-tech rail transit tool that uses electromagnetic force to achieve train suspension and guidance, and uses superconducting magnetic levitation technology to break away from the ground and eliminate friction resistance. The near-vacuum pipeline inside greatly reduces air resistance, allowing the maximum speed to reach a subsonic speed of over 1,000 kilometers per hour.
[0003] Wireless energy transmission high-frequency cables are the core basic components and key equipment of subsonic vacuum tube flying cars and high-speed magnetic levitation. They are used inside tube flying cars and high-speed magnetic levitation as non-contact power transmission devices to receive power transmitted by electromagnetic fields on the track. Since they need to be in a space where strong and weak electric signals are intertwined and alternating electromagnetic fields for a long time, the heat of the cables themselves is prone to accumulate, causing the wireless energy transmission system to operate at high temperatures for a long time. Therefore, it is of great significance to develop high-frequency wireless energy transmission cable sheath materials that are highly conductive, resistant to bending, resistant to stress relaxation, and flame-retardant to ensure that subsonic vacuum tube flying cars can operate under ultra-high-speed conditions.
[0004] There is a technical gap in the domestic wireless power transmission high-frequency cables for subsonic vacuum tube flying cars. Judging from the current research and development progress of various countries, they are all in the research and development stage. 1,000 kilometers per hour is the current design speed of vacuum tube flying cars. When the technology matures, the speed level will inevitably increase significantly, and the maximum speed is expected to reach 4,000 kilometers per hour. In the future, vacuum tube flying cars will inevitably exceed the speed of sound and eventually exceed Mach 3, and wireless power transmission high-frequency cables for vacuum tube flying cars will also develop in the direction of lower loss and higher performance. Therefore, it is of great significance to develop high-frequency wireless power transmission cable sheath materials that are highly conductive, resistant to bending, resistant to stress relaxation, and flame-retardant for subsonic vacuum tube flying cars. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide a high-conductivity, bending-resistant, stress-relaxation-resistant, flame-retardant wireless energy transmission high-frequency cable sheath material for subsonic vacuum pipeline flying cars, as well as a preparation method and application thereof.
[0006] The present invention adopts the following technical solutions to solve the above technical problems:
[0007] A sheath material for a wireless power transmission high-frequency cable, comprising the following raw materials in parts by weight: 100-150 parts of ethylene-vinyl acetate copolymer (EVA), 10-30 parts of rubber, 10-30 parts of a compatibilizer, 10-15 parts of an ionic flame retardant cross-linking sensitizer, 30-50 parts of a conductive filler, 80-130 parts of an inorganic smoke suppressant flame retardant, 10-15 parts of a phosphorus flame retardant, 10-15 parts of a vulcanizing agent, 2-5 parts of a vulcanization accelerator, 0.5-2 parts of an antioxidant, and 0.5-2 parts of an antioxidant;
[0008] Wherein, the ionic flame retardant cross-linking sensitizer is an ionic liquid containing a phenylphosphonic acid unit, and the structure is shown in the following formula I:
[0009]
[0010] The inorganic smoke suppressant flame retardant is a mixture of nano-sized aluminum hydroxide, magnesium hydroxide, zinc borate, talcum powder and mica flakes;
[0011] The conductive filler is polyaniline and ethylene-methacrylate ionomer / Zn 2+ mixture.
[0012] As one of the preferred embodiments of the present invention, the VA mass content in the ethylene-vinyl acetate copolymer (EVA) is 28-40%, and the density is 0.95-1.02 g / cm 3 The melting point is 58-75°C, and the melt flow rate is 0.5-300g / 10min at 190°C / 2.16kg.
[0013] As one of the preferred embodiments of the present invention, the combined rubber is at least two of EPDM rubber, butadiene rubber, and natural rubber, with a Shore hardness (A) of 45 to 80 and a melt flow rate of 3 to 19 g / 10 min at 230°C / 2.16 kg. More preferably, it is a mixture of EPDM rubber, butadiene rubber, and natural rubber.
[0014] As one of the preferred embodiments of the present invention, the compatibilizer is one or more of maleic anhydride grafted polyethylene, maleic anhydride grafted polypropylene, maleic anhydride grafted ethylene-vinyl acetate, and glycidyl methacrylate grafted ethylene-octene copolymer. More preferably, it is a mixture of maleic anhydride grafted polyethylene, maleic anhydride grafted polypropylene, maleic anhydride grafted ethylene-vinyl acetate, and glycidyl methacrylate grafted ethylene-octene copolymer.
[0015] As one of the preferred embodiments of the present invention, the phosphorus-based flame retardant is one or more of ammonium polyphosphate, tri-o-cresyl phosphate, and diammonium hydrogen phosphate, and more preferably a mixture of multiple types of ammonium polyphosphate, tri-o-cresyl phosphate, and diammonium hydrogen phosphate.
[0016] As one of the preferred embodiments of the present invention, the vulcanizing agent is one or more of dicumyl peroxide and dibenzoyl peroxide, and more preferably a mixture of dicumyl peroxide and dibenzoyl peroxide.
[0017] As one of the preferred embodiments of the present invention, the vulcanization accelerator is one or more of 2-mercaptobenzothiazole, triallyl isocyanurate, and zinc oxide, and more preferably a mixture of 2-mercaptobenzothiazole, triallyl isocyanurate, and zinc oxide.
[0018] As one of the preferred embodiments of the present invention, the antioxidant is one or more of 2-methyl-1,2-diphenylacetophenone, 4'4-dimethyldiphenylethane, and 4'4-dimethylstilbene, and more preferably a mixture of 2-methyl-1,2-diphenylacetophenone, 4'4-dimethyldiphenylethane, and 4'4-dimethylstilbene.
[0019] As one of the preferred embodiments of the present invention, the antioxidant is one or more of 2-mercaptobenzoimidazole, 2,6-di-tert-butyl-4-methylphenol, and 2,2,4-trimethyl-1,2-dihydroquinoline. More preferably, it is a mixture of 2-mercaptobenzoimidazole, 2,6-di-tert-butyl-4-methylphenol, and 2,2,4-trimethyl-1,2-dihydroquinoline.
[0020] A method for preparing the above-mentioned wireless energy transmission high-frequency cable sheath material, comprising the following steps: adding ethylene-vinyl acetate copolymer, rubber and compatibilizer to a high-speed mixer and mixing to obtain a premix; taking half of the premix and adding it to an internal mixer and mixing evenly; at the same time, adding the other half of the premix and an ionic flame retardant cross-linking sensitizer, a conductive filler, an inorganic smoke suppressant flame retardant, a phosphorus flame retardant, an anti-aging agent and an antioxidant to the mixer and mixing them, and then adding the premix to the internal mixer to which half of the premix has been added for melt blending; after cooling and drying, placing the premix in a twin-screw extruder for melt blending and extrusion, and cooling and drying to obtain a blended masterbatch; adding the blended masterbatch, a vulcanizing agent and a vulcanization accelerator to a high-speed mixer, mixing, placing the premix in a twin-screw extruder for melt blending and extrusion, and cooling and drying to obtain a pre-crosslinked masterbatch; placing the pre-crosslinked masterbatch in a wire and cable extruder for melt extrusion to obtain a pre-crosslinked cable; and finally, irradiating the pre-crosslinked cable product.
[0021] As one of the preferred embodiments of the present invention, first, ethylene-vinyl acetate copolymer, rubber and compatibilizer are added into a high-speed mixer and mixed at 1500-3000 rpm for 5 minutes to obtain a premix;
[0022] Then, half of the premix is added to an internal mixer, melt blended at 100° C. and 50 rpm for 3 minutes, and mixed evenly; at the same time, the other half of the premix is added to a high-speed mixer according to a corresponding proportion with an ionic flame retardant cross-linking sensitizer, a conductive filler, an inorganic smoke suppressant flame retardant, a phosphorus flame retardant, an antioxidant, and an antioxidant, mixed at 1500-3000 rpm for 5 minutes, and then added to an internal mixer, melt blended at 100° C. and 50 rpm for 10 minutes; after cooling and drying, the mixture is placed in a twin-screw extruder at a temperature of 100-140° C. for melt blending and extrusion, and a blended masterbatch is obtained after cooling and drying;
[0023] The above blended masterbatch, vulcanizing agent and vulcanization accelerator are added into a high-speed mixer, mixed at 2000-4000 rpm for 10 min, then placed in a twin-screw extruder at a temperature of 135-155° C. for melt blending and extrusion, and cooled and dried to obtain a pre-crosslinked masterbatch;
[0024] Then, the masterbatch is placed in a wire and cable extruder at a temperature of 145 to 160° C. for melt extrusion to obtain a pre-crosslinked cable;
[0025] Finally, it was irradiated for 20 minutes under the conditions of beam voltage of 2-3 MeV, beam current of 30 mA, and irradiation dose of 350 kGy to obtain a finished cable.
[0026] As one of the preferred embodiments of the present invention, the method further comprises the step of preparing the ionic flame retardant cross-linking sensitizer:
[0027] 3-Methyl-2-pyridinecarboxylic acid is mixed with acetone, and heated and stirred to react with pentaerythritol triallyl ether under the action of a catalyst; after the reaction, the reaction liquid is cooled, filtered, separated, and dried to obtain the product MCA-HICA, the structure of which is shown in Formula II:
[0028]
[0029] After MCA-HICA and phenylphosphonic acid are mixed, acetone is added to dissolve, and the mixture is heated and stirred under a nitrogen atmosphere for reaction; after the reaction is completed, the mixture is washed and dried to obtain an ionic flame retardant cross-linking sensitizer shown in Formula I:
[0030]
[0031] As one of the preferred embodiments of the present invention, the preparation steps of the ionic flame retardant cross-linking sensitizer are specifically as follows:
[0032] 3-Methyl-2-pyridinecarboxylic acid is mixed with acetone, and heated and stirred with pentaerythritol triallyl ether at 70°C for 8 hours under the catalytic action of H2SO4; after the reaction, the reaction liquid is cooled, filtered, separated, and dried to obtain the product MCA-HICA, the structure of which is shown in Formula II:
[0033]
[0034] MCA-HICA and phenylphosphonic acid were mixed in a round-bottom flask, acetone was added to dissolve, and the mixture was heated to 50° C. in an oil bath under a nitrogen atmosphere and stirred for 24 hours. After the reaction, the mixture was washed three times with acetone and dried to obtain an ionic flame retardant cross-linking sensitizer as shown in Formula I:
[0035]
[0036] An application of a sheath material for a wireless power transmission high-frequency cable made of fir, characterized in that the sheath material for a wireless power transmission high-frequency cable is applied to cables for vacuum tube flying cars with a speed of 1,000 kilometers per hour or more and cables for intelligent equipment serving in complex environments such as magnetic levitation trains.
[0037] The advantages of the present invention compared to the prior art are:
[0038] (1) The conductive filler of the present invention can inhibit the radial and tangential diffusion movement of electrons in the polymer phase and at the interface, eliminate the interface polarization, electronic polarization and dipole steering polarization, release the carriers enriched on the surface of the material, promote the interface bonding between the organic-inorganic filler and the polymer matrix, and greatly improve the conductive properties of the material;
[0039] (2) The inorganic smoke suppressant flame retardant of the present invention improves the flame retardancy and smoke suppression performance, and the lamellar inorganic particles can act as a dispersant for the nano inorganic particles to improve their dispersibility in the polymer matrix and improve the dimensional stability of the material;
[0040] (3) The ionic flame retardant crosslinking sensitizer of the present invention contains rich vinyl and pyridine. As an inorganic filler surface modifier, it can significantly improve the interfacial compatibility between the inorganic filler and the polymer matrix, and promote the synergistic crosslinking of the matrix during the crosslinking process. At the same time, it contains a large amount of phosphorus and nitrogen elements. During the combustion process, it can be used as an intumescent flame retardant to improve the flame retardant properties of the material, and has excellent thermal stability, carbonization performance and flame retardant properties;
[0041] (4) The present invention can improve the uniform dispersion of fillers in the matrix through step-by-step blending; at the same time, the ionic cross-linking sensitizer further improves the dispersibility of the inorganic filler and promotes the cross-linking degree of the polymer matrix. The interpenetrating network formed between the fillers forms a natural barrier layer during combustion; the introduction of the conductive filler promotes the interfacial bonding between the organic / inorganic filler and the polymer matrix, and uses electron beam irradiation to construct multiple chemical cross-linking structures to form a dual network structure of an organic-inorganic hybrid network and a multi-scale conductive enhancer carrier release network, which further restricts the movement of the molecular chain and improves the bending resistance and stress relaxation resistance of the material. DETAILED DESCRIPTION
[0042] The following is a detailed description of an embodiment of the present invention. This embodiment is implemented on the premise of the technical solution of the present invention, and a detailed implementation method and a specific operation process are given, but the protection scope of the present invention is not limited to the following embodiment.
[0043] About the raw materials used in the following examples:
[0044] Ethylene-vinyl acetate copolymer (EVA): density is 0.951g / cm 3 The melt index is 3g / 10min under the test conditions of 190℃ / 2.16kg, the VA content is 28%, the tensile strength is 29MPa, the elongation at break is 800-1000%, and EVA265 from DuPont of the United States is selected.
[0045] Rubber used: a mixture of EPDM rubber, butadiene rubber and natural rubber in a mass ratio of 4:1:1; wherein the EPDM rubber Mooney viscosity [ML1+4,125°C] is 31, the ethylene content is 44%, the propylene content is 57%, the vinylidene-norbornene content is 1%, and EPDM 430 of DuPont Company of the United States is selected.
[0046] Compatibilizer: a mixture of maleic anhydride grafted polyethylene (PE-g-MAH), maleic anhydride grafted polypropylene (PP-g-MAH), maleic anhydride grafted ethylene-vinyl acetate (EVA-g-MAH), and glycidyl methacrylate grafted ethylene-octene copolymer (POE-g-GMA) in a mass ratio of 1:1:1:3; among which PE-g-MAH is DuPont E588 from the United States, PP-g-MAH is Arkema 18722 from France, EVA-g-MAH is LyondellBasell PX1008, and POE-g-GMA is sog-03 from Jiayirong Polymer (Shanghai) Co., Ltd.
[0047] Ionic flame retardant cross-linking sensitizer: an ionic liquid containing phenylphosphonic acid moieties, the preparation method is as follows:
[0048] 21.48 g of 3-methyl-2-pyridinecarboxylic acid was mixed with 500 mL of acetone, and heated and stirred with 40.16 g of pentaerythritol triallyl ether at 70° C. for 8 h under the catalytic action of H2SO4; after the reaction, the reaction liquid was cooled, filtered, separated, and dried to obtain 52.94 g of MCA-HICA represented by formula II:
[0049]
[0050] 52.94 g of MCA-HICA and 10 g of phenylphosphonic acid were mixed in a round-bottom flask, and 750 ml of acetone was added to dissolve. The mixture was heated to 50° C. in an oil bath under a nitrogen atmosphere and stirred for reaction for 24 h. After the reaction, the mixture was washed three times with acetone and dried to obtain 53.5 g of an ionic flame retardant cross-linking sensitizer represented by formula I:
[0051]
[0052] Inorganic smoke suppressant flame retardant: a mixture of nano-grade aluminum hydroxide, magnesium hydroxide, zinc borate, and high specific surface area and high silicon content talc and mica flakes in a mass ratio of 8:8:1:1:1; the raw materials are all selected from Jinan Taixing Fine Chemical Co., Ltd.
[0053] Conductive fillers: polyaniline, ethylene methacrylate ionomer / Zn 2+ A mixture of 1:1 by mass ratio; wherein polyaniline is selected from Merck, Germany, ethylene-methacrylate ionomer / Zn 2+ Selected for use in Shanghai MacLean Biochemical Technology Co., Ltd.
[0054] Phosphorus-based flame retardant: a mixture of ammonium polyphosphate, tri-o-cresyl phosphate, and diammonium hydrogen phosphate in a mass ratio of 1:1:1; the raw materials are all selected from Shanghai Aladdin Biochemical Technology Co., Ltd.
[0055] Curing agent: a mixture of dicumyl peroxide and dibenzoyl peroxide in a mass ratio of 1:1; the raw materials are all selected from Shanghai MacLean Biochemical Technology Co., Ltd.
[0056] Vulcanization accelerator: a mixture of 2-mercaptobenzothiazole, triallyl isocyanurate, and zinc oxide in a mass ratio of 1:1:3; the raw materials are all from Shanghai Aladdin Biochemical Technology Co., Ltd.
[0057] Antiaging agent: a mixture of 2-methyl-1,2-diphenylacetophenone, 4'4-dimethyldiphenylethane and 4'4-dimethylstilbene in a mass ratio of 1:1:1; the raw materials are all from Merck, Germany.
[0058] Antioxidant: a mixture of 2-mercaptobenzoimidazole, 2,6-di-tert-butyl-4-methylphenol and 2,2,4-trimethyl-1,2-dihydroquinoline in a mass ratio of 1:1:1; all raw materials are from Merck, Germany.
[0059] Table 1 Raw material formula of sheath materials of Examples 1 to 6 and Comparative Examples 1 to 6 (unit: parts by weight)
[0060]
[0061]
[0062] Example 1
[0063] A wireless power transmission high frequency cable sheath material of this embodiment, the raw materials and formula are shown in Table 1.
[0064] Preparation method:
[0065] (1) First, ethylene-vinyl acetate copolymer, rubber and compatibilizer are added to a high-speed mixer and mixed at 1500 rpm for 5 minutes to obtain a premix.
[0066] (2) Take half of the premix and add it to an internal mixer, melt blend it at 100°C and 50 rpm for 3 minutes, and mix it evenly; at the same time, add the other half of the premix and ionic flame retardant cross-linking sensitizer, conductive filler, inorganic smoke suppressant flame retardant, phosphorus flame retardant, antioxidant, and antioxidant into a high-speed mixer in corresponding proportions, mix it at 1500 rpm for 5 minutes, add it to the internal mixer, melt blend it at 100°C and 50 rpm for 10 minutes; after cooling and drying, place it in a twin-screw extruder at a temperature of 100°C for melt blending and extrusion, and obtain the blended masterbatch after cooling and drying.
[0067] (3) The above-mentioned blended masterbatch, vulcanizing agent and vulcanization accelerator are added into a high-speed mixer, mixed at 2000 rpm for 10 min, and then placed in a twin-screw extruder at a temperature of 135° C. for melt blending and extrusion, and cooled and dried to obtain a pre-crosslinked masterbatch.
[0068] (4) placing the masterbatch in a wire and cable extruder at a temperature of 145° C. for melt extrusion to obtain a pre-crosslinked cable.
[0069] (5) The pre-crosslinked cable was irradiated for 20 minutes under the conditions of a beam voltage of 2 MeV, a beam current of 30 mA, and an irradiation dose of 350 kGy to obtain a finished cable.
[0070] Example 2
[0071] A wireless power transmission high frequency cable sheath material of this embodiment, the raw materials and formula are shown in Table 1.
[0072] Preparation method:
[0073] (1) First, ethylene-vinyl acetate copolymer, rubber and compatibilizer are added to a high-speed mixer and mixed at 2000 rpm for 5 minutes to obtain a premix.
[0074] (2) Take half of the premix and add it to an internal mixer, melt blend it at 100°C and 50 rpm for 3 minutes, and mix it evenly; at the same time, add the other half of the premix and ionic flame retardant cross-linking sensitizer, conductive filler, inorganic smoke suppressant flame retardant, phosphorus flame retardant, antioxidant, and antioxidant into a high-speed mixer in corresponding proportions, mix it at 2000 rpm for 5 minutes, add it to the internal mixer, melt blend it at 100°C and 50 rpm for 10 minutes; after cooling and drying, place it in a twin-screw extruder at a temperature of 120°C for melt blending and extrusion, and obtain the blended masterbatch after cooling and drying.
[0075] (3) The above-mentioned blended masterbatch, vulcanizing agent and vulcanization accelerator are added into a high-speed mixer, mixed at 3000 rpm for 10 min, and then placed into a twin-screw extruder at a temperature of 145° C. for melt blending and extrusion, and cooled and dried to obtain a pre-crosslinked masterbatch.
[0076] (4) placing the masterbatch in a wire and cable extruder at a temperature of 155° C. for melt extrusion to obtain a pre-crosslinked cable.
[0077] (5) The pre-crosslinked cable was irradiated for 20 minutes under the conditions of a beam voltage of 2.5 MeV, a beam current of 30 mA, and an irradiation dose of 350 kGy to obtain a finished cable.
[0078] Example 3
[0079] A wireless power transmission high frequency cable sheath material of this embodiment, the raw materials and formula are shown in Table 1.
[0080] Preparation method:
[0081] (1) First, ethylene-vinyl acetate copolymer, rubber and compatibilizer are added to a high-speed mixer and mixed at 3000 rpm for 5 minutes to obtain a premix.
[0082] (2) Take half of the premix and add it to an internal mixer, melt blend it at 100°C and 50 rpm for 3 minutes, and mix it evenly; at the same time, add the other half of the premix and ionic flame retardant cross-linking sensitizer, conductive filler, inorganic smoke suppressant flame retardant, phosphorus flame retardant, antioxidant, and antioxidant into a high-speed mixer in corresponding proportions, mix it at 3000 rpm for 5 minutes, add it to the internal mixer, melt blend it at 100°C and 50 rpm for 10 minutes; after cooling and drying, place it in a twin-screw extruder at a temperature of 140°C for melt blending and extrusion, and obtain the blended masterbatch after cooling and drying.
[0083] (3) The above-mentioned blended masterbatch, vulcanizing agent and vulcanization accelerator are added into a high-speed mixer, mixed at 4000 rpm for 10 min, and then placed into a twin-screw extruder at a temperature of 155° C. for melt blending and extrusion, and cooled and dried to obtain a pre-crosslinked masterbatch.
[0084] (4) placing the masterbatch in a wire and cable extruder at a temperature of 160° C. for melt extrusion to obtain a pre-crosslinked cable.
[0085] (5) The pre-crosslinked cable was irradiated for 20 minutes under the conditions of a beam voltage of 3 MeV, a beam current of 30 mA, and an irradiation dose of 350 kGy to obtain a finished cable.
[0086] Example 4
[0087] A wireless power transmission high frequency cable sheath material of this embodiment, the raw materials and formula are shown in Table 1.
[0088] Preparation method:
[0089] (1) First, ethylene-vinyl acetate copolymer, rubber and compatibilizer are added to a high-speed mixer and mixed at 2000 rpm for 5 minutes to obtain a premix.
[0090] (2) Take half of the premix and add it to an internal mixer, melt blend it at 100°C and 50 rpm for 3 minutes, and mix it evenly; at the same time, add the other half of the premix and ionic flame retardant cross-linking sensitizer, conductive filler, inorganic smoke suppressant flame retardant, phosphorus flame retardant, antioxidant, and antioxidant into a high-speed mixer in corresponding proportions, mix it at 2000 rpm for 5 minutes, add it to the internal mixer, melt blend it at 100°C and 50 rpm for 10 minutes; after cooling and drying, place it in a twin-screw extruder at a temperature of 120°C for melt blending and extrusion, and obtain the blended masterbatch after cooling and drying.
[0091] (3) The above-mentioned blended masterbatch, vulcanizing agent and vulcanization accelerator are added into a high-speed mixer, mixed at 3000 rpm for 10 min, and then placed into a twin-screw extruder at a temperature of 145° C. for melt blending and extrusion, and cooled and dried to obtain a pre-crosslinked masterbatch.
[0092] (4) placing the masterbatch in a wire and cable extruder at a temperature of 155° C. for melt extrusion to obtain a pre-crosslinked cable.
[0093] (5) The pre-crosslinked cable was irradiated for 20 minutes under the conditions of a beam voltage of 2.5 MeV, a beam current of 30 mA, and an irradiation dose of 350 kGy to obtain a finished cable.
[0094] Example 5
[0095] A wireless power transmission high frequency cable sheath material in this embodiment, the raw materials and formula are shown in Table 1, and the preparation method is the same as that in Example 4.
[0096] Example 6
[0097] A wireless power transmission high frequency cable sheath material in this embodiment, the raw materials and formula are shown in Table 1, and the preparation method is the same as that in Example 4.
[0098] Comparative Example 1
[0099] A cable sheath material in this comparative example, the raw materials and formula are shown in Table 1, and the preparation method is the same as Example 4.
[0100] Comparative Example 2
[0101] A cable sheath material in this comparative example, the raw materials and formula are shown in Table 1, and the preparation method is the same as Example 4.
[0102] Comparative Example 3
[0103] A cable sheath material in this comparative example, the raw materials and formula are shown in Table 1, and the preparation method is the same as Example 4.
[0104] Comparative Example 4
[0105] A cable sheath material in this comparative example, the raw materials and formula are shown in Table 1, and the preparation method is the same as Example 4.
[0106] Comparative Example 5
[0107] A cable sheath material in this comparative example, the raw materials and formula are shown in Table 1, and the preparation method is the same as Example 4.
[0108] Comparative Example 6
[0109] A cable sheath material of this comparative example, raw materials and formula are shown in Table 1.
[0110] Preparation method:
[0111] (1) EVA, rubber, compatibilizer, ionic flame retardant cross-linking sensitizer, conductive filler, inorganic smoke suppressant flame retardant, phosphorus flame retardant, vulcanizer, vulcanization accelerator, antioxidant, and antioxidant are added to an internal mixer in proportion, melt blended at 100° C. and 50 rpm for 10 min, cooled and dried, and then placed in a twin-screw extruder for melt blending and extrusion, and cooled and dried to obtain a blended masterbatch.
[0112] (2) placing the masterbatch in a wire and cable extruder at a temperature of 155° C. for melt extrusion to obtain a pre-crosslinked cable.
[0113] (3) The pre-crosslinked cable was irradiated for 20 minutes under the conditions of a beam voltage of 2.5 MeV, a beam current of 30 mA, and an irradiation dose of 350 kGy to obtain the finished cable.
[0114] The main performance indicators of the cable sheath materials prepared in the above Examples 1-6 and Comparative Examples 1-6 are shown in Table 2.
[0115] Table 2 Performance test results of various embodiments and comparative examples
[0116]
[0117]
[0118]
[0119] From Table 2, we can see that:
[0120] Since the ionic cross-linking sensitizer contains rich vinyl and pyridine units, it can effectively promote the formation of the cross-linking network inside the material and the organic-inorganic hybrid network, and improve the strength of the material. The introduction of inorganic smoke suppressant flame retardant containing high specific surface area talc and mica flakes ensures the uniform dispersion of the filler in the polymer matrix, improves the dimensional stability and smoke suppression performance of the material, and plays a synergistic flame retardant role with the ionic cross-linking sensitizer. In addition, the introduction of conductive fillers promotes the interface bonding between organic / inorganic fillers and polymer matrix, and constructs multiple chemical cross-linking structures through electron beam irradiation. The dual network structure of organic-inorganic hybrid network and multi-scale conductive enhancer carrier release network can further restrict the movement of molecular chains and improve the conductivity, bending resistance and stress relaxation resistance of the material. Step-by-step blending is adopted, and the shearing action between different melt strength gradients leads to the migration of fillers, and the dispersion state of fillers is directional regulated, and finally excellent comprehensive performance is obtained.
[0121] Compared with Example 5, Comparative Example 1 introduces the phosphorus-based flame retardant "phenylphosphonic acid" and the traditional conductive filler "polyaniline and carbon black", combined with the "hydroxide flame retardant", and does not add the ionic cross-linking sensitizer and conductive filler provided by the present invention, resulting in poor flame retardancy and conductivity of the material, which is difficult to meet the use requirements of the vacuum pipeline flying car in a complex environment. Compared with Example 5, Comparative Example 2 adds the ionic flame retardant cross-linking sensitizer and conductive filler provided by the present invention to construct a multiple chemical cross-linking structure, which can effectively improve the mechanical and conductive properties of the material, but does not introduce the inorganic smoke suppressant flame retardant provided by the present invention, resulting in poor flame retardancy and smoke suppression properties of the material. Compared with Example 5, Comparative Example 3 adds the inorganic smoke suppressant flame retardant and conductive filler provided by the present invention as an inorganic filler, which can effectively improve the flame retardancy of the material, and at the same time, the rich rigid elements can enhance the mechanical properties of the material, but does not introduce the ionic flame retardant cross-linking sensitizer, resulting in poor overall performance of the material. Compared with Example 5, Comparative Example 4 introduces a large amount of flame retardants, conductive fillers and inorganic smoke suppressant flame retardants, which makes it difficult to disperse the fillers evenly, thereby reducing the interaction between the fillers and the polymer matrix. Compared with Example 5, Comparative Example 5 adds the ionic flame retardant cross-linking sensitizer and inorganic smoke suppressant flame retardant provided by the present invention, but does not introduce conductive fillers, resulting in poor conductivity, bending resistance and stress relaxation resistance of the material. In summary, the superiority of the formula designed by the present invention is reflected. In addition, Comparative Example 6 has the same formula system as Example 5, but the processing technology is different. The traditional one-step blending is used, which leads to poor dispersion of inorganic fillers and difficulty in constructing a uniform organic-inorganic hybrid network, reflecting the superiority of the preparation process of the present invention.
[0122] Combined with the above data analysis, it can be seen that the performance of the cable sheath material of the present invention is greatly improved. There are several reasons: (1) The ionic flame retardant cross-linking sensitizer contains rich vinyl and pyridine units, which act as cross-linking sensitizers and dispersants to improve the strength of the material. (2) The introduction of conductive fillers inhibits the radial and tangential diffusion movement of electrons in the polymer phase and at the interface, eliminates the polarization of the interface and releases the carriers enriched on the surface of the material, promotes the interface bonding between the organic / inorganic filler and the polymer matrix, and greatly improves the conductivity of the material. (3) Multiple chemical cross-linking structures are constructed through radiation cross-linking to form a dual network structure of organic-inorganic hybrid network and multi-scale conductive enhancer carrier release network, which limits the movement of molecular chain segments and plays a role in bending resistance and stress relaxation resistance. (4) The cross-linking structure can effectively prevent the material from swelling in oil and improve oil resistance. In addition, the large number of double bonds in the ionic flame retardant cross-linking sensitizer can effectively prevent material aging and improve the performance of the material after aging test. (5) Specific processing technology leads to uniform dispersion of fillers, enhances the efficiency of free radical generation during irradiation, and improves the cross-linking degree of the material compared to the traditional one-step method.
[0123] The present invention synthesizes an ionic flame retardant cross-linking sensitizer with a specific structure, and introduces an EVA composite material by compounding it with an inorganic smoke suppressant flame retardant and a conductive filler. The comprehensive performance of the material is improved through radiation cross-linking, and the problem of bending and stress relaxation of traditional materials under high stress conditions, which leads to a rapid decline in performance of the cable under actual operating conditions, is overcome. The long-term stable operation of the cable under high temperature, high stress and strong torsion environment is achieved, and the material and related technologies are applied to cables for subsonic vacuum pipeline flying cars and related intelligent equipment.
[0124] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A sheath material for a wireless power transmission high frequency cable, characterized in that: The invention comprises the following raw materials in parts by weight: 100-150 parts of ethylene-vinyl acetate copolymer, 10-30 parts of rubber, 10-30 parts of compatibilizer, 10-15 parts of ionic flame retardant cross-linking sensitizer, 30-50 parts of conductive filler, 80-130 parts of inorganic smoke suppressant flame retardant, 10-15 parts of phosphorus flame retardant, 10-15 parts of vulcanizing agent, 2-5 parts of vulcanization accelerator, 0.5-2 parts of antioxidant, and 0.5-2 parts of antioxidant; Wherein, the ionic flame retardant cross-linking sensitizer is an ionic liquid containing a phenylphosphonic acid unit, and the structure is shown in the following formula I: The inorganic smoke suppressant flame retardant is a mixture of nano-sized aluminum hydroxide, magnesium hydroxide, zinc borate, talcum powder and mica flakes; The conductive filler is polyaniline and ethylene-methacrylate ionomer / Zn 2+ mixture.
2. The sheath material for wireless power transmission high frequency cable according to claim 1, characterized in that: The combined rubber is at least two of EPDM rubber, butadiene rubber and natural rubber.
3. The sheath material for wireless power transmission high frequency cable according to claim 1, characterized in that: The compatibilizer is one or more of maleic anhydride grafted polyethylene, maleic anhydride grafted polypropylene, maleic anhydride grafted ethylene-vinyl acetate, and glycidyl methacrylate grafted ethylene-octene copolymer.
4. The sheath material for wireless power transmission high frequency cable according to claim 1, characterized in that: The phosphorus-based flame retardant is one or more of ammonium polyphosphate, tri-o-cresyl phosphate, and diammonium hydrogen phosphate.
5. The sheath material for wireless power transmission high frequency cable according to claim 1, characterized in that: The vulcanizing agent is one or more of dicumyl peroxide and dibenzoyl peroxide; the vulcanization accelerator is one or more of 2-mercaptobenzothiazole, triallyl isocyanurate and zinc oxide.
6. The sheath material for wireless power transmission high frequency cable according to claim 1, characterized in that: The antioxidant is one or more of 2-methyl-1,2-diphenylacetophenone, 4'4-dimethyldiphenylethane, and 4'4-dimethylstilbene.
7. The sheath material for wireless power transmission high frequency cable according to claim 1, characterized in that: The antioxidant is one or more of 2-thiol benzoimidazole, 2,6-di-tert-butyl-4-methylphenol, and 2,2,4-trimethyl-1,2-dihydroquinoline.
8. A method for preparing a sheath material for a wireless power transmission high frequency cable according to any one of claims 1 to 7, characterized in that: Add ethylene-vinyl acetate copolymer, rubber and compatibilizer into a high-speed mixer to obtain a premix; take half of the premix and add it into an internal mixer to mix evenly; at the same time, add the other half of the premix and ionic flame retardant cross-linking sensitizer, conductive filler, inorganic smoke suppressant flame retardant, phosphorus flame retardant, antioxidant and antioxidant into the mixer and mix them, then add them into the internal mixer to which half of the premix has been added for melt blending; after cooling and drying, place them into a twin-screw extruder for melt blending and extrusion, and obtain a blended masterbatch after cooling and drying; add the above blended masterbatch, vulcanizing agent and vulcanization accelerator into a high-speed mixer, mix them, place them into a twin-screw extruder for melt blending and extrusion, and obtain a pre-crosslinked masterbatch after cooling and drying; The pre-crosslinked masterbatch is placed in a wire and cable extruder for melt extrusion to obtain a pre-crosslinked cable; Finally, after irradiation, the finished cable is obtained.
9. The method for preparing the sheath material of the wireless power transmission high frequency cable according to claim 8, characterized in that: The method also includes the steps of preparing the ionic flame retardant cross-linking sensitizer: 3-Methyl-2-pyridinecarboxylic acid is mixed with acetone, and heated and stirred to react with pentaerythritol triallyl ether under the action of a catalyst; after the reaction, the reaction liquid is cooled, filtered, separated, and dried to obtain the product MCA-HICA, the structure of which is shown in Formula II: After MCA-HICA and phenylphosphonic acid are mixed, acetone is added to dissolve, and the mixture is heated and stirred under a nitrogen atmosphere for reaction; after the reaction is completed, the mixture is washed and dried to obtain an ionic flame retardant cross-linking sensitizer shown in Formula I:
10. An application of the sheath material for wireless power transmission high frequency cables as claimed in any one of claims 1 to 7, characterized in that: The wireless energy transmission high-frequency cable sheath material is applied to cables for vacuum tube flying cars with a speed of 1,000 kilometers per hour or more and cables for magnetic levitation trains.