Polypropylene composite material as well as preparation method and application thereof

Through the synergy between low-melting point polybutene modified hollow glass microbeads and chopped glass fibers, the problem that polypropylene materials are difficult to achieve low density and high bending modulus in automotive applications is solved, and the polypropylene composite materials are realized. Low density and high flexural modulus, suitable for the lightweight needs of automotive parts.

CN118931031AActive Publication Date: 2024-11-12JIANGSU KINGFA SCI & TECH ADVANCED MATERIALS CO LTD +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202310535598.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-12
Publication Date
2024-11-12
Estimated Expiration
2043-05-12

AI Technical Summary

Technical Problem

It is difficult for existing polypropylene materials to achieve both low density and high flexural modulus, especially under the demand for lightweight automobiles. The existing enhancement methods lead to an increase in density, making it difficult to take into account both.

Method used

By using low-melting polybutene to modify hollow glass microbeads and chopped glass fibers, low-melting polybutene pre-covers glass microbeads, reducing the breakage rate and increasing the material modulus, controlling glass fibers and modified microbes Bead feeding timing to achieve low density and high flexural modulus.

Benefits of technology

The low density and high flexural modulus of polypropylene composite materials are achieved, with a density of no more than 0.988g/cm3 and a flexural modulus of up to 3500MPa, which is suitable for the lightweight needs of automotive parts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004226033830000021
    Figure BDA0004226033830000021
  • Figure BDA0004226033830000051
    Figure BDA0004226033830000051
  • Figure BDA0004226033830000061
    Figure BDA0004226033830000061
Patent Text Reader

Abstract

The invention discloses a polypropylene composite material as well as a preparation method and application thereof, and belongs to the technical field of high polymer materials. The polypropylene composite material is mainly prepared from the following components in parts by weight: 40-80 parts of polypropylene resin; 10 to 30 parts of chopped glass fiber; 10-30 parts of modified hollow glass beads; 0.4 to 1.2 parts of a processing aid; wherein the modified hollow glass beads are formed by modifying hollow glass beads with low-melting-point polybutylene. The low-melting-point polybutylene is used for preparing the modified hollow glass beads in advance, and the modified hollow glass beads and the glass fibers have a synergistic effect, so that low density and high bending modulus are realized at the same time. According to the polypropylene composite material, the density does not exceed 0.988 g / cm < 3 > and can be as low as 0.921 g / cm < 3 >, and the bending modulus can reach 3500 MPa or above and can reach 4500 MPa.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of polymer materials, and more specifically to a polypropylene composite material and a preparation method and application thereof. Background Art

[0002] Polypropylene material has the characteristics of low density, chemical resistance and excellent cost performance, and has been widely used in all parts of automotive interior and exterior.

[0003] With the development of new energy materials for lightweight demand, the application of polypropylene materials in automobiles has received more attention, so polypropylene needs to be modified to meet different performance requirements. The current common modification method is to enhance its scratch resistance, rigidity and creep resistance by adding glass fiber, talcum powder, calcium carbonate, wollastonite, whiskers and other materials. However, the above processing methods of polypropylene composites will cause the density to increase, which does not meet the development trend of lightweight automobiles.

[0004] Hollow glass microspheres are used in many material fields, such as fillers for thermal insulation materials, cable insulation materials, etc. Hollow glass microsphere products have high dimensional stability and do not produce orientation and warping. However, when hollow glass microspheres are used in modified plastics, the shearing of the twin screws causes the hollow glass microspheres to break, especially when the density of glass fiber reinforced polypropylene materials is reduced, which does not achieve the ideal effect.

[0005] The prior art discloses a polypropylene composite material, comprising 44-75 parts of polypropylene with an isotacticity greater than 90%, 10-20 parts of low isotactic polypropylene with an isotacticity of 30-60%, 10-30 parts of hollow glass microspheres, 13 parts of thermoplastic hollow polymer microspheres and 3-4 parts of processing aids. After a certain proportion of low isotactic polypropylene is introduced into the matrix material, the low isotactic polypropylene can be quickly coated on the surface of the hollow glass microspheres to prevent the hollow glass microspheres from being squeezed and broken. Moreover, the polypropylene composite material has a lower density and is lighter. However, after glass fiber reinforcement is added to the system, the breakage of the hollow glass microspheres will increase. Although the modulus can be improved, the density will increase, so it is difficult to achieve low density and high bending modulus at the same time. Summary of the invention

[0006] The technical problem to be solved by the present invention is to overcome the defects and shortcomings of existing polypropylene that it is difficult to achieve low density and high bending modulus at the same time, and to provide a polypropylene composite material that achieves low density and high bending modulus at the same time through the synergistic effect of specific modified hollow glass microspheres and chopped glass fibers.

[0007] Another object of the present invention is to provide a method for preparing a polypropylene composite material.

[0008] Another object of the present invention is to provide an application of a polypropylene composite material in the preparation of automobile interiors or automobile exteriors.

[0009] Another object of the present invention is to provide an automobile component.

[0010] The above-mentioned purpose of the present invention is achieved through the following technical solutions:

[0011] A polypropylene composite material is mainly prepared from the following components by weight:

[0012]

[0013] The modified hollow glass microspheres are formed by low-melting-point polybutene-modified hollow glass microspheres, the melting point of the low-melting-point polybutene is less than or equal to 100° C., the structure of the low-melting-point polybutene-modified hollow glass microspheres is a core-shell structure, and the low-melting-point polybutene is coated on the surface of the glass microspheres.

[0014] The present invention achieves low density and high bending modulus by using low melting point polybutene to prepare the modified hollow glass microspheres in advance and the synergistic effect of the chopped glass fibers. This is because the early coating of the low melting point polybutene improves the reduction of the breakage rate of the hollow microspheres and ensures the improvement of the material modulus.

[0015] The melting point of low-melting-point polybutene directly affects the density of the material. Too high a melting point will affect the coating effect of polybutene on the glass microspheres, which is not conducive to reducing the density.

[0016] Preferably, the weight ratio of the chopped glass fibers to the modified hollow glass microspheres is (0.3-3):1.

[0017] Preferably, the weight ratio of the chopped glass fibers to the modified hollow glass microspheres is (0.5-2.2):1.

[0018] Optionally, in the modified hollow glass microspheres, the weight ratio of the low melting point polybutene to the hollow glass microspheres is (0.2-1.6):1.

[0019] Preferably, in the modified hollow glass microspheres, the weight ratio of the low melting point polybutene to the hollow glass microspheres is (0.6-1):1.

[0020] Optionally, the melting point of the low-melting-point polybutene is 88-96° C., and the testing standard is ISO 11357-3-2011.

[0021] Preferably, the melting point of the low-melting-point polybutene is 90-94° C., and the testing standard is ISO 11357-3-2011.

[0022] Optionally, the melt mass flow rate of the low melting point polybutene is 40 to 800 g / 10 min, the test standard is GB / T 3682.1-2018, and the test conditions are 190° C. and 2.16 kg.

[0023] Preferably, the melt mass flow rate of the low melting point polybutene is 40 to 100 g / 10 min, the test standard is GB / T 3682.1-2018, and the test conditions are 190° C. and 2.16 kg.

[0024] Optionally, the average particle size of the hollow glass microspheres is 20 to 50 μm.

[0025] Preferably, the average particle size of the hollow glass microspheres is 20 to 30 μm.

[0026] Preferably, the true density of the hollow glass microspheres is 0.35 to 0.64 g / cm 3 .

[0027] Preferably, the true density of the hollow glass microspheres is 0.38 to 0.46 g / cm 3 .

[0028] Optionally, the average retention length of the chopped glass fibers is 400-600 μm. The test method for the average retention length is: ISO 22314-2006.

[0029] Preferably, the average retention length of the chopped glass fibers is 530-550 μm. The test method for the average retention length is: ISO 22314-2006.

[0030] Preferably, the average diameter of the chopped glass fibers is 12-15 μm.

[0031] Optionally, the melt mass flow rate of the polypropylene resin is 10 to 150 g / 10 min, the test standard is GB / T 3682.1-2018, and the test conditions are 230° C. and 2.16 kg.

[0032] Preferably, the melt mass flow rate of the polypropylene resin is 30 to 100 g / 10 min, the test standard is GB / T 3682.1-2018, and the test conditions are 230° C. and 2.16 kg.

[0033] Preferably, the polypropylene resin is homopolypropylene.

[0034] Preferably, the processing aid comprises an antioxidant and / or a lubricant.

[0035] The antioxidant is one or more of a hindered phenol antioxidant, a phosphite antioxidant or a phosphite antioxidant.

[0036] Optionally, the hindered phenol antioxidant is a fully hindered phenol: one or more of antioxidants 1010, 1076 or AO-330.

[0037] Optionally, the phosphite antioxidant is one or more of phosphites: antioxidant 168, 626 or PEP-36.

[0038] Optionally, the weight ratio of the hindered phenol antioxidant to the phosphite antioxidant is (0.5-1.0):1.

[0039] Optionally, the weight ratio of the hindered phenol antioxidant to the phosphite antioxidant is (0.8-1.0):1.

[0040] Antioxidants can improve the antioxidant effect of polypropylene composites.

[0041] Lubricants can improve the lubrication effect of polypropylene composites.

[0042] Preferably, the lubricant is ethylene bisstearamide.

[0043] Preferably, the weight portion of the antioxidant is 0.2 to 2 parts; the weight portion of the lubricant is 0.2 to 1.0 parts.

[0044] The invention also protects a preparation method of a polypropylene composite material, comprising the following steps: mixing the components, melting and extruding through a twin-screw extruder, granulating, and drying to obtain the polypropylene composite material.

[0045] The preparation method of the polypropylene composite material of the present invention can be prepared by the following steps:

[0046] S1. The low melting point polybutene resin and hollow glass microspheres are mixed and extruded to obtain modified hollow glass microspheres;

[0047] S2. The polypropylene resin, antioxidant and lubricant are mixed and added to the extruder from the main feed port of the extruder, and the chopped glass fibers and the modified hollow glass microspheres are added to the extruder from the side feed port of the extruder, and the polypropylene composite material is obtained after melt extrusion, granulation and drying;

[0048] Among them, in S2, the chopped glass fibers are added to the extruder from the fourth to the sixth screw of the extruder;

[0049] The modified hollow glass microspheres are added into the extruder from the seventh to the ninth screw of the extruder.

[0050] Preferably, the extruder is a twin-screw extruder.

[0051] In the present invention, by controlling the timing of adding chopped glass fibers and modified hollow glass microspheres, it is beneficial to control the average retention length of glass fibers in the polypropylene composite material and reduce the breakage of hollow glass microspheres in the polypropylene system, thereby achieving low density and high bending modulus at the same time.

[0052] The polypropylene composite material prepared by the present invention has low density and high bending modulus, and can be widely used in the preparation of plastic products. The present invention particularly protects the use of the polypropylene composite material in the preparation of automobile parts, especially automobile interiors and / or automobile exteriors.

[0053] Optionally, the automobile exterior may be components such as a bumper bracket and a tailgate inner panel.

[0054] An automobile component is made by injection molding any one of the above-mentioned polypropylene composite materials.

[0055] Preferably, the automotive component is an automotive interior.

[0056] The automobile interior decoration includes components such as door panels and instrument panel frames.

[0057] Compared with the prior art, the present invention has the following beneficial effects:

[0058] The polypropylene composite material of the present invention comprises polypropylene resin, chopped glass fibers, modified hollow glass microspheres and processing aids. The present invention achieves low density and high bending modulus by using low melting point polybutene to prepare the modified hollow glass microspheres in advance and the synergistic effect of the chopped glass fibers. DETAILED DESCRIPTION

[0059] The present invention is further described below in conjunction with specific embodiments, but the embodiments do not limit the present invention in any form. Unless otherwise specified, the raw materials and reagents used in the embodiments of the present invention are conventionally purchased raw materials and reagents.

[0060] The raw materials used in the embodiments and comparative examples of the present invention are shown in Table 1 below.

[0061] Table 1

[0062]

[0063] The self-made chopped glass fibers 3 and 4 were obtained by purchasing Taishan continuous fiber EDR300-T738, and then cutting them into chopped fibers with lengths of 9.0 mm and 2.0 mm using scissors.

[0064] The preparation method of modified hollow glass microspheres is as follows:

[0065] The low melting point polybutene resin and hollow glass microspheres are mixed, extruded and granulated in a single screw extruder to obtain modified hollow glass microspheres; the machine temperature is set at 160° C. and the screw speed is 250 rpm.

[0066] The composition of the modified hollow glass microspheres is shown in Table 2 below.

[0067] Table 2

[0068] Modified hollow glass microspheres 1 Hollow glass microspheres1 Low melting point polybutene 1 The weight ratio of low melting point polybutene and hollow glass microspheres is 1 Modified hollow glass microspheres 2 Hollow glass microspheres 2 Low melting point polybutene 1 The weight ratio of low melting point polybutene and hollow glass microspheres is 1 Modified hollow glass microspheres 3 Hollow glass microspheres 3 Low melting point polybutene 1 The weight ratio of low melting point polybutene and hollow glass microspheres is 1 Modified hollow glass microspheres 4 Hollow glass microspheres1 Low melting point polybutene 2 The weight ratio of low melting point polybutene and hollow glass microspheres is 1 Modified hollow glass microspheres 5 Hollow glass microspheres1 High melting point polybutene 3 The weight ratio of high melting point polybutene to hollow glass microspheres is 1 Modified hollow glass microspheres 6 Hollow glass microspheres1 Low melting point polybutene 1 The weight ratio of low melting point polybutene to hollow glass microspheres is 0.2 Modified hollow glass microspheres 7 Hollow glass microspheres1 Low melting point polybutene 1 The weight ratio of low melting point polybutene to hollow glass microspheres is 0.6 Modified hollow glass microspheres 8 Hollow glass microspheres1 Low melting point polybutene 1 The weight ratio of low melting point polybutene to hollow glass microspheres is 1.6 Modified hollow glass microspheres 9 Hollow glass microspheres1 Low melting point polypropylene The weight ratio of low melting point polypropylene and hollow glass microspheres is 1

[0069] Examples 1 to 21

[0070] A polypropylene composite material is prepared from the following components by weight: polypropylene resin; short-cut glass fibers; modified hollow glass microspheres; a lubricant; and an antioxidant.

[0071] The specific content of each component is shown in Table 3 below.

[0072] Table 3 Composition of polypropylene composite materials in various embodiments (by weight)

[0073] Components 1 2 3 4 5 Polypropylene resin 1 59.3 40 80 54.3 59.3 Chopped glass fiber1 20 30 10 15 27 Modified hollow glass microspheres 1 20 30 10 30 13 Antioxidants 0.4 2 0.2 0.4 0.4 Lubricants 0.3 1 0.2 0.3 0.3

[0074] Table 3

[0075]

[0076]

[0077] Table 3

[0078] Components 14 15 16 17 18 19 20 21 22 Polypropylene resin 1 59.3 59.3 59.3 59.3 59.3 59.3 59.3 59.3 59.3 Chopped glass fiber1 20 20 20 20 20 20 10 30 20 Modified hollow glass microspheres 1 30 10 20 Modified hollow glass microspheres 2 20 Modified hollow glass microspheres 3 20 Modified hollow glass microspheres 4 20 Modified hollow glass microspheres 6 20 Modified hollow glass microspheres 7 20 Modified hollow glass microspheres 8 20 Antioxidants 0.4 0.4 0.4 0.4 0.4 0.4 0.4 0.4 0.4 Lubricants 0.3 0.3 0.3 0.3 0.3 0.3 0.3 0.3 0.3

[0079] The preparation method of the polypropylene composite material comprises the following steps:

[0080] Add polypropylene resin, antioxidant and lubricant into a high mixer and mix for 3 minutes, add them into the twin-screw extruder from the main feeding port of the twin-screw extruder for melting, mixing and dispersion, add short-cut glass fibers into the twin-screw extruder from the side feeding port of the twin-screw extruder, add modified hollow glass microbeads into the twin-screw extruder from the side feeding port of the twin-screw extruder, and obtain the polypropylene composite material after melt extrusion, granulation and drying;

[0081] The length-to-diameter ratio of the twin-screw extruder is 40:1; the twin-screw extruder has 10 barrel sections; the screw speed is 350 rpm; the processing temperatures from the feed port to the die are: 100°C, 180°C, 180°C, 180°C, 180°C, 180°C, 180°C, 180°C, 180°C, 180°C;

[0082] Among them, the chopped glass fibers are added into the twin-screw extruder in the fifth barrel;

[0083] The modified hollow glass microspheres are added into the twin-screw extruder in the eighth screw barrel.

[0084] Embodiment 22

[0085] A polypropylene composite material, the formula is the same as that of Example 1, and the difference from Example 1 is the preparation method:

[0086] Add polypropylene resin, antioxidant and lubricant into a high mixer and mix for 3 minutes, add them into the twin-screw extruder from the main feeding port of the twin-screw extruder for melting, mixing and dispersion, add short-cut glass fibers into the twin-screw extruder from the side feeding port of the twin-screw extruder, add modified hollow glass microbeads into the twin-screw extruder from the side feeding port of the twin-screw extruder, and obtain the polypropylene composite material after melt extrusion, granulation and drying;

[0087] The length-to-diameter ratio of the twin-screw extruder is 40:1; the twin-screw extruder has 10 barrel sections; the screw speed is 350 rpm; the processing temperatures from the feed port to the die are: 100°C, 180°C, 180°C, 180°C, 180°C, 180°C, 180°C, 180°C, 180°C, 180°C;

[0088] Among them, the chopped glass fibers are added into the twin-screw extruder in the eighth barrel;

[0089] The modified hollow glass microspheres are added into the twin-screw extruder in the fifth screw barrel.

[0090] Comparative Example 1

[0091] A polypropylene composite material, which is different from Example 1 in that glass fibers and modified hollow glass microspheres 1 are not added.

[0092] The preparation method of the polypropylene composite material is the same as that in Example 1, which will not be described again.

[0093] Comparative Example 2

[0094] A polypropylene composite material is prepared from the following components by weight: 1 polypropylene resin; 1 short glass fiber; 1 low melting point polybutene; 1 hollow glass microsphere; a lubricant; and an antioxidant, wherein the amount of each component used is the same as that in Example 1.

[0095] The preparation method of the polypropylene composite material is basically the same as that of Example 1, except that:

[0096] Adding low melting point polybutene 1 and hollow glass microspheres 1 into the twin-screw extruder from the side feed port of the twin-screw extruder;

[0097] The low melting point polybutene 1 and the hollow glass microspheres 1 are added into the twin-screw extruder in the eighth screw barrel.

[0098] Comparative Examples 3 to 7

[0099] A polypropylene composite material is prepared from the following components by weight: polypropylene resin; short-cut glass fibers; modified hollow glass microspheres; a lubricant; and an antioxidant.

[0100] The specific content of each component is shown in Table 4 below.

[0101] Table 4 Composition of polypropylene composite materials of each comparative example (by weight)

[0102] Components 3 4 5 6 7 Polypropylene resin 1 59.3 59.3 59.3 59.3 59.3 Chopped glass fiber1 20 0 40 20 Modified hollow glass microspheres 1 80 40 0 Modified hollow glass microspheres 9 20 Modified hollow glass microspheres 5 20 Antioxidants 0.4 0.4 0.4 0.4 0.4 Lubricants 0.3 0.3 0.3 0.4 0.3

[0103] The preparation method of the polypropylene composite material is the same as that of Example 1.

[0104] Results

[0105] The polypropylene composite materials of each embodiment and comparative example were tested according to the following method:

[0106] (1) Density: Standard: ISO-1183-2006; 23°C / 50% humidity.

[0107] (2) Flexural modulus: Standard: ISO-178-2006; 23°C / 50% humidity.

[0108] (3) Average retention length of glass fiber: Standard: ISO 22314-2006, unit: μm.

[0109] The specific test results of the polypropylene composite materials of each embodiment are described in Table 5 below:

[0110] Table 5

[0111]

[0112] Table 5

[0113]

[0114]

[0115] The specific test results of the polypropylene composite materials of each comparative example are described in Table 6 below:

[0116] Table 6

[0117] Comparative Example 1# 2# 3# 4# 5# 6# 7# <![CDATA[Density / g / cm 3 > 0.900 0.997 0.968 0.856 1.21 1.034 1.022 Flexural modulus / MPa 1900 4300 3450 3000 6000 4450 4450 Glass fiber retention length / 525 532 / 544 521 523

[0118] From the above data, it can be seen that the polypropylene composite material of the present invention achieves low density and high bending modulus at the same time through the synergistic effect of the hollow glass microspheres prepared in advance by low melting point polybutene and short chopped glass fibers. The density of the polypropylene composite material of the present invention does not exceed 0.988g / cm 3 , can be as low as 0.921g / cm 3 , the flexural modulus can reach over 3500MPa and up to 4500MPa.

[0119] It can be seen from Comparative Example 1 that without adding chopped carbon fibers and modified hollow glass microspheres 1, the bending modulus of the material is too low to meet the requirements.

[0120] It can be seen from Comparative Example 2 that the low-melting-point polybutene 1 and the hollow glass microspheres 1 are not reacted in advance to prepare the modified hollow glass microspheres, and the density of the material is too high, and there is no good effect of reducing the density.

[0121] It can be seen from Comparative Example 3 that the amount of modified hollow glass microspheres used is too much, the density of the material is not significantly reduced, and the modulus is lower than 3500 MPa.

[0122] It can be seen from Comparative Example 4 that low density can be achieved by adding only modified hollow glass microspheres without adding chopped glass fibers, but the material modulus is lower than 3500 MPa.

[0123] It can be seen from Comparative Example 5 that low density cannot be achieved by adding only chopped glass fibers without adding modified hollow glass microspheres.

[0124] It can be seen from Comparative Example 6 that the modified hollow glass microspheres are made of hollow glass microspheres modified with low-melting-point polypropylene. Under the same processing technology, the low-melting-point polypropylene modified masterbatch cannot achieve low density.

[0125] It can be seen from Examples 1, 4, 5, 20 and 21 that the smaller the weight ratio of the chopped glass fibers to the modified hollow glass microspheres, the lower the density of the material.

[0126] It can be seen from Examples 1 and 6 to 10 that when the melt mass flow rate of the polypropylene resin is 30 to 60 g / 10 min, the material density is lower, and the density will increase when the melt index is slightly higher or lower.

[0127] It can be seen from Example 1 and Example 11 to Example 13 that the average retention length of the chopped fibers is 530-550 μm, which is more conducive to reducing the density.

[0128] It can be seen from Example 1 and Example 14 to Example 15 that the smaller the average particle size of the hollow glass microspheres, the more conducive it is to reducing the density.

[0129] It can be seen from Example 1, Example 16 and Comparative Example 7 that the melting point of the low-melting-point polybutene is optimal when it is 90-94°C. When the melting point is higher than 100°C, the density is too high.

[0130] It can be seen from Example 1 and Example 17 to Example 19 that when the weight of low melting point polybutene and hollow glass microspheres is (0.6 to 1):1, the density of the material is lower and the modulus of the material is higher.

[0131] It can be seen from Examples 1 and 22 that the feeding method in Example 1 is more conducive to achieving low density and high modulus than the conventional section in which the chopped glass fibers and modified hollow glass microspheres are added in Example 24.

[0132] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the embodiments of the present invention. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.

Claims

1. A polypropylene composite material, characterized in that: By weight, it includes the following components: The modified hollow glass microspheres are formed by low-melting-point polybutene-modified hollow glass microspheres, the melting point of the low-melting-point polybutene is less than or equal to 100° C., the structure of the low-melting-point polybutene-modified hollow glass microspheres is a core-shell structure, and the low-melting-point polybutene is coated on the surface of the glass microspheres.

2. The polypropylene composite material according to claim 1, characterized in that: The weight ratio of the chopped glass fibers to the modified hollow glass microspheres is (0.3-3):

1.

3. The polypropylene composite material according to claim 1, characterized in that: In the modified hollow glass microspheres, the weight ratio of the low melting point polybutene to the hollow glass microspheres is (0.2-1.6):

1.

4. The polypropylene composite material according to claim 1, characterized in that: The melting point of the low-melting-point polybutene is 90° C. to 94° C., the test standard is ISO 11357-3-2011, the melt mass flow rate of the low-melting-point polybutene is 40 to 800 g / 10 min, the test standard is GB / T 3682.1-2018, and the test conditions are 190° C. and 2.16 kg.

5. The polypropylene composite material according to claim 1, characterized in that: The average particle size of the hollow glass microspheres is 20 to 50 μm.

6. The polypropylene composite material according to claim 1, characterized in that: The average retention length of the chopped glass fibers is 400-600 μm, and the average diameter of the chopped glass fibers is 12-15 μm.

7. The polypropylene composite material according to claim 1, characterized in that: The melt mass flow rate of the polypropylene resin is 10 to 150 g / 10 min, the test standard is GB / T 3682.1-2018, and the test conditions are 230° C. and 2.16 kg.

8. The polypropylene composite material according to claim 1, characterized in that: The processing aid comprises an antioxidant and / or a lubricant; the antioxidant is a hindered phenol antioxidant and / or a phosphite antioxidant; the lubricant is an ethylene bisstearic acid amide; the weight portion of the antioxidant is 0.2 to 2 parts; the weight portion of the lubricant is 0.2 to 1.0 parts.

9. The method for preparing the polypropylene composite material according to any one of claims 1 to 8, characterized in that: The steps include: S1. The low melting point polybutene resin and hollow glass microspheres are mixed and extruded to obtain modified hollow glass microspheres; S2. The polypropylene resin, antioxidant and lubricant are mixed and added to the extruder from the main feed port of the extruder, and the chopped glass fibers and the modified hollow glass microspheres are added to the extruder from the side feed port of the extruder, and the polypropylene composite material is obtained after melt extrusion, granulation and drying; Among them, in S2, the chopped glass fibers are added to the extruder from the fourth to the sixth screw of the extruder; The modified hollow glass microspheres are added into the extruder from the seventh to the ninth screw of the extruder.

10. Use of the polypropylene composite material according to any one of claims 1 to 8 in the preparation of automotive interior or exterior materials.

Citation Information

Patent Citations

  • Glass fiber reinforced modified polypropylene material and preparation method thereof

    CN105367897A

  • Low-floating-fiber continuous long glass fiber reinforced polypropylene composite material and preparation method and application thereof

    CN110041609A

  • Low-density, high-rigidity and high-toughness polypropylene composite material and preparation method thereof

    CN110655718A

  • Thermoplastic polymer compositions with improved flexibility

    WO2020260428A1