Wear-resistant plastic material and preparation method thereof
By using modified silica and carbon fiber fusion fillers in plastic materials, combined with dodecyl dimethylbenzyl ammonium chloride, the wear problem of traditional plastic materials in high friction environments is solved, and wear resistance is significantly improved and tensile properties, extending service life.
Patent Information
- Application Number
- CN202411183881.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-12
AI Technical Summary
Traditional plastic materials are prone to wear, scratches and other problems in high friction and high load environments, resulting in a shortened service life.
Using a mototropic filler including silica and carbon fiber, the hydrophobicity and binding properties are improved by modification treatment, and combined with dodecyl dimethylbenzyl ammonium chloride, added to polypropylene to form a wear-resistant plastic material .
It significantly improves the wear resistance and tensile properties of plastic materials, reduces wear rate and sticking risks, and extends service life.
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of plastic material preparation, and in particular to a wear-resistant plastic material and a preparation method thereof. Background Art
[0002] Plastic raw materials are made of high molecular synthetic resin (polymer) as the main component, infiltrated with various auxiliary materials or additives. Under specific temperature and pressure, they have plasticity and fluidity, can be molded into a certain shape, and maintain the same shape under certain conditions.
[0003] Plastic materials are widely used in many fields due to their advantages such as light weight, easy processing and corrosion resistance. However, traditional plastic materials have obvious deficiencies in wear resistance, especially in high-friction and high-load environments, prone to wear and scratches, which seriously affect the service life of the product. Summary of the invention
[0004] In order to improve the wear resistance of plastic materials, the present application provides a wear-resistant plastic material and a preparation method thereof.
[0005] In the first aspect, the present application provides a wear-resistant plastic material, which adopts the following technical solution: A wear-resistant plastic material comprises the following raw materials in parts by mass: 100-120 parts of polypropylene, 5-10 parts of friction-increasing filler, 1-3 parts of polyol ester, and 1-3 parts of calcium stearate; the friction-increasing filler comprises silicon dioxide.
[0006] By adopting the above technical solution, adding the friction-increasing filler made of silicon dioxide to the plastic material can improve the wear resistance of the plastic material. The specific reasons are as follows: Silicon dioxide can form rough and sharp protrusions on the surface of plastic materials, increase the friction coefficient, increase the surface roughness of the plastic material, and thus increase the wear resistance of the plastic material.
[0007] Preferably, the friction-increasing filler also includes carbon fiber.
[0008] By adopting the above technical solution, the carbon fiber itself has the characteristics of high strength and high modulus, so adding the carbon fiber to the plastic material can significantly improve the wear resistance of the plastic material.
[0009] In addition, carbon fiber can improve the thermal conductivity of plastic materials, thereby improving the diffusion efficiency of heat generated on the friction surface, thereby reducing the temperature of the friction surface, reducing adhesion to the plastic material, further reducing the wear rate, and thus improving the structural stability and thermal stability of the plastic material.
[0010] In addition, carbon fiber has a flaky polycrystalline graphite structure, which allows carbon fiber to act as a lubricant in the system, effectively improving the flow properties of the plastic material and reducing the possibility of the plastic material sticking to the inner wall of the equipment during molding.
[0011] And because the adhesion between silica and polypropylene is a physical interaction, it is difficult for the phase interface to effectively combine, thereby reducing the tensile properties of the plastic material. Carbon fiber can play a bridging role, which can increase the effective bonding between silica and polypropylene, so that the tensile properties of the plastic material can be improved.
[0012] Preferably, the mass ratio of silica to carbon fiber is 1:(3.12-3.34).
[0013] By adopting the above technical solution, the mass ratio of silicon dioxide to carbon fiber is controlled within the above range, which can effectively improve the wear resistance of the friction-increasing filler to the plastic material.
[0014] Preferably, the modified preparation method of silicon dioxide comprises the following steps: Add silicon dioxide to anhydrous ethanol, stir evenly, then add deionized water and ammonia water, stir again, add dodecyltriethoxysilane, heat to react, wash and dry in sequence after the reaction is completed to obtain modified silicon dioxide.
[0015] By adopting the above technical scheme, dodecyltriethoxysilane is hydrolyzed and grafted onto the surface of silica, thereby reducing the hydroxyl content on the surface of silica and reducing the surface energy of silica, so that the surface contact angle of silica increases, thereby improving the hydrophobicity of silica, so that the modified silica can form a protective film on the surface of the plastic material, thereby reducing the direct contact between the plastic material and external substances, thereby reducing the wear of the surface of the plastic material, and effectively improving the wear resistance of the plastic material.
[0016] Preferably, the mass ratio of silicon dioxide to dodecyltriethoxysilane is 1:(0.6-0.8).
[0017] By adopting the above technical solution and controlling the mass ratio of carbon fiber to dodecyltriethoxysilane within the above range, the hydrophobicity of silica can be effectively improved.
[0018] Preferably, the modification preparation method of the carbon fiber comprises the following steps: The carbon fiber, polymethylhydrogensiloxane and deionized water are mixed and then subjected to homogeneous reaction. After the reaction is complete, the mixture is cooled to room temperature, and then filtered and dried in sequence to obtain the modified carbon fiber.
[0019] By adopting the above technical scheme, polymethylhydrogensiloxane is used to hydrophobically modify the carbon fiber, thereby improving the hydrophobicity of the carbon fiber, so that the modified carbon fiber can form a protective film on the surface of the plastic material, thereby reducing the direct contact between the plastic material and external substances, thereby reducing the wear on the surface of the plastic material and effectively improving the wear resistance of the plastic material.
[0020] Preferably, the mass ratio of the carbon fiber to polymethylhydrogensiloxane is 1:(0.2-0.4).
[0021] By adopting the above technical solution and controlling the mass ratio of carbon fiber to polymethylhydrogensiloxane within the above range, the hydrophobicity of the carbon fiber can be effectively improved.
[0022] Preferably, 1-3 parts of dodecyldimethylbenzylammonium chloride are also included.
[0023] By adopting the above technical solution, dodecyl dimethyl benzyl ammonium chloride is a cationic surfactant, which contains positive charges in its molecular structure. Therefore, it can electrically neutralize the negative charges on the surface of modified silica and modified carbon fiber, thereby enhancing the adsorption effect between modified silica and modified carbon fiber, thereby improving the wear resistance and tensile properties of plastic materials.
[0024] In addition, dodecyl dimethyl benzyl ammonium chloride can reduce the surface tension of the plastic material matrix, making it easier for silica and carbon fibers to be evenly dispersed in the plastic matrix, thereby forming a closer bond between the various components of the plastic material.
[0025] In a second aspect, the present application provides a method for preparing a wear-resistant plastic material as in the first aspect, which adopts the following technical solution: A method for preparing a wear-resistant plastic material comprises the following steps: After the polypropylene and the friction-increasing filler are mixed evenly, the polyol ester and calcium stearate are added and mixed evenly again to obtain a mixture; the mixture is then extruded and formed, and finally the extrudate is cooled, pelletized and packaged in sequence to obtain a plastic material.
[0026] In summary, the present application includes at least one of the following beneficial technical effects: 1. Silicon dioxide can form rough and sharp protrusions on the surface of plastic materials, increase the friction coefficient, increase the surface roughness of the plastic material, and thus increase the wear resistance of the plastic material.
[0027] 2. Dodecyltriethoxysilane is hydrolyzed and grafted onto the surface of silica, thereby reducing the hydroxyl content on the surface of silica and the surface energy of silica, so that the surface contact angle of silica increases, thereby improving the hydrophobicity of silica, reducing the wear on the surface of the plastic material, and effectively improving the wear resistance of the plastic material. DETAILED DESCRIPTION
[0028] The present application is further described in detail below in conjunction with the embodiments and comparative examples. The raw materials involved in the present application can all be obtained commercially, among which polypropylene is provided by Shanghai MacLean Biochemical Technology Co., Ltd., dodecyltriethoxysilane is provided by Shanghai Shiyang Chemical Co., Ltd., polymethylhydrogensiloxane is provided by Jinan Longcheng Silicone Co., Ltd., and dodecyldimethylbenzylammonium chloride is provided by Chengdu Zero Six Biotechnology Co., Ltd.
[0029] Example 1 The wear-resistant plastic material includes the following raw materials: 110 g of polypropylene, 8 g of friction-increasing filler, 2 g of polyol ester, and 2 g of calcium stearate.
[0030] The friction-increasing filler includes silica.
[0031] The preparation method of the wear-resistant plastic material comprises the following steps: Put polypropylene and friction-increasing filler into a high-speed mixer and mix them evenly. Then put polyol ester and calcium stearate into the high-speed mixer and mix them evenly again to obtain a mixture. Then pour the mixture into a twin-screw extruder for extrusion molding. Finally, cool the extrudate with circulating water at 10°C, cut into pellets and package to obtain a plastic material.
[0032] Example 2 The wear-resistant plastic material includes the following raw materials: 100g of polypropylene, 5g of friction-increasing filler, 1g of polyol ester, and 1g of calcium stearate.
[0033] The friction-increasing filler includes silica and carbon fiber, and the mass ratio of silica to carbon fiber is 1:3.12.
[0034] The method for preparing the friction-increasing filler comprises the following steps: The silica and the carbon fiber are mixed and stirred evenly to prepare a friction-increasing filler.
[0035] The preparation method of the wear-resistant plastic material comprises the following steps: Put polypropylene and friction-increasing filler into a high-speed mixer and mix them evenly. Then put polyol ester and calcium stearate into the high-speed mixer and mix them evenly again to obtain a mixture. Then pour the mixture into a twin-screw extruder for extrusion molding. Finally, cool the extrudate with circulating water at 10°C, cut into pellets and package to obtain a plastic material.
[0036] Example 3 The wear-resistant plastic material includes the following raw materials: 120g of polypropylene, 10g of friction-increasing filler, 3g of polyol ester, and 3g of calcium stearate.
[0037] The friction-increasing filler includes silica and carbon fiber, and the mass ratio of silica to carbon fiber is 1:3.34.
[0038] The method for preparing the friction-increasing filler comprises the following steps: The silica and the carbon fiber are mixed and stirred evenly to prepare a friction-increasing filler.
[0039] The preparation method of the wear-resistant plastic material comprises the following steps: Put polypropylene and friction-increasing filler into a high-speed mixer and mix them evenly. Then put polyol ester and calcium stearate into the high-speed mixer and mix them evenly again to obtain a mixture. Then pour the mixture into a twin-screw extruder for extrusion molding. Finally, cool the extrudate with circulating water at 10°C, cut into pellets and package to obtain a plastic material.
[0040] Example 4 The wear-resistant plastic material includes the following raw materials: 110 g of polypropylene, 8 g of friction-increasing filler, 2 g of polyol ester, and 2 g of calcium stearate.
[0041] The friction-increasing filler includes silica and carbon fiber, and the mass ratio of silica to carbon fiber is 1:3.23.
[0042] The method for preparing the friction-increasing filler comprises the following steps: The silica and the carbon fiber are mixed and stirred evenly to prepare a friction-increasing filler.
[0043] The preparation method of the wear-resistant plastic material comprises the following steps: Put polypropylene and friction-increasing filler into a high-speed mixer and mix them evenly. Then put polyol ester and calcium stearate into the high-speed mixer and mix them evenly again to obtain a mixture. Then pour the mixture into a twin-screw extruder for extrusion molding. Finally, cool the extrudate with circulating water at 10°C, cut into pellets and package to obtain a plastic material.
[0044] Example 5 The difference between Example 5 and Example 4 is that the mass ratio of silicon dioxide to carbon fiber is 1:2.92.
[0045] Example 6 The difference between Example 6 and Example 4 is that the mass ratio of silicon dioxide to carbon fiber is 1:3.54.
[0046] Example 7 The difference between Example 7 and Example 4 is that the modified preparation method of silicon dioxide comprises the following steps: Add 1g of silica to 15g of anhydrous ethanol, stir evenly, then add 2g of deionized water and 3g of ammonia water, stir vigorously for 30min, then add 0.6g of dodecyltriethoxysilane, and react at 80°C for 6h. After the reaction, wash the product three times with anhydrous ethanol by centrifugation, and then dry the product in vacuum at 60°C for 12h to obtain modified silica.
[0047] Example 8 The difference between Example 8 and Example 4 is that the modified preparation method of silicon dioxide comprises the following steps: Add 1g of silica to 15g of anhydrous ethanol, stir evenly, then add 2g of deionized water and 3g of ammonia water, stir vigorously for 30min, then add 0.8g of dodecyltriethoxysilane, and react at 80°C for 6h. After the reaction, wash the product three times with anhydrous ethanol by centrifugation, and then dry the product at 60°C in vacuum for 12h to obtain modified silica.
[0048] Example 9 The difference between Example 9 and Example 4 is that the modified preparation method of silicon dioxide comprises the following steps: Add 1g of silica to 15g of anhydrous ethanol, stir evenly, then add 2g of deionized water and 3g of ammonia water, stir vigorously for 30min, then add 0.7g of dodecyltriethoxysilane, and react at 80°C for 6h. After the reaction, wash the product three times with anhydrous ethanol by centrifugation, and then dry the product in vacuum at 60°C for 12h to obtain modified silica.
[0049] Example 10 The difference between Example 10 and Example 9 is that the mass ratio of silicon dioxide to dodecyltriethoxysilane is 1:0.4.
[0050] Embodiment 11 The difference between Example 11 and Example 9 is that the mass ratio of silicon dioxide to dodecyltriethoxysilane is 1:1.
[0051] Example 12 The difference between Example 12 and Example 9 is that the modification preparation method of carbon fiber includes the following steps: Add 20g carbon fiber, 4g polymethylhydrogensiloxane and 75g deionized water into a polytetrafluoroethylene liner, seal the liner and put it into the stainless steel shell of the reactor, and put the reactor into the homogeneous reactor. The rotation rate of the homogeneous reactor is 60r / min. After heating to 130°C, keep the constant temperature for 2h. After the reaction is completed, stop rotating and cool to 25°C. Then filter and dry the slurry in the liner to obtain modified carbon fiber.
[0052] Example 13 The difference between Example 13 and Example 9 is that the modification preparation method of carbon fiber includes the following steps: Add 20g carbon fiber, 8g polymethylhydrogensiloxane and 75g deionized water into a polytetrafluoroethylene liner, seal the liner and put it into the stainless steel shell of the reactor, and put the reactor into the homogeneous reactor. The rotation rate of the homogeneous reactor is 60r / min. After heating to 130°C, keep the constant temperature for 2h. After the reaction is completed, stop rotating and cool to 25°C. Then filter and dry the slurry in the liner to obtain modified carbon fiber.
[0053] Embodiment 14 The difference between Example 14 and Example 9 is that the modification preparation method of carbon fiber includes the following steps: Add 20g carbon fiber, 6g polymethylhydrogensiloxane and 75g deionized water into a polytetrafluoroethylene liner, seal the liner and put it into the stainless steel shell of the reactor, and put the reactor into the homogeneous reactor. The rotation rate of the homogeneous reactor is 60r / min. After heating to 130°C, keep the constant temperature for 2h. After the reaction is completed, stop rotating and cool to 25°C. Then filter and dry the slurry in the liner to obtain modified carbon fiber.
[0054] Embodiment 15 The difference between Example 15 and Example 14 is that the mass ratio of carbon fiber to polymethyl hydrogen siloxane is 1:0.1.
[0055] Example 16 The difference between Example 16 and Example 14 is that the mass ratio of carbon fiber to polymethyl hydrogen siloxane is 1:0.5.
[0056] Embodiment 17 The difference between Example 17 and Example 14 is that the wear-resistant plastic material further includes 1g of dodecyldimethylbenzylammonium chloride.
[0057] The preparation method of the wear-resistant plastic material comprises the following steps: Put polypropylene and friction-increasing filler into a high-speed mixer and mix them evenly. Then put polyol ester, calcium stearate and dodecyl dimethyl benzyl ammonium chloride into the high-speed mixer and mix them evenly again to obtain a mixture. Then pour the mixture into a twin-screw extruder for extrusion molding. Finally, cool the extrudate with circulating water at 10°C, cut into pellets and package to obtain a plastic material.
[0058] Embodiment 18 The difference between Example 18 and Example 17 is that the wear-resistant plastic material also includes 3g of dodecyldimethylbenzylammonium chloride.
[0059] Embodiment 19 The difference between Example 19 and Example 17 is that the wear-resistant plastic material also includes 2g of dodecyldimethylbenzylammonium chloride.
[0060] Comparative Example 1 The difference between Comparative Example 1 and Example 1 is that the wear-resistant plastic material does not contain friction-increasing filler.
[0061] That is, the preparation method of the wear-resistant plastic material comprises the following steps: Polypropylene, polyol ester, calcium stearate and dodecyl dimethyl benzyl ammonium chloride are put into a high-speed mixer and mixed until uniform to obtain a mixture; the mixture is then poured into a twin-screw extruder for extrusion molding; finally, the extrudate is cooled with circulating water at 10° C., pelletized and packaged to obtain a plastic material.
[0062] Comparative Example 2 The difference between Comparative Example 2 and Example 1 is that the friction-increasing filler includes carbon fiber.
[0063] Performance testing: The plastic materials prepared in Examples 1-19 and Comparative Examples 1-2 were sampled and subjected to the following performance tests: 1. Wear resistance: Refer to GB / T1689-2014 "Determination of wear resistance of vulcanized rubber (using Akron abrasion tester)" to test the wear volume, and record the test results in Table 1, where the smaller the wear volume, the better the wear resistance.
[0064] 2. Tensile properties: Refer to GB / T528-2009 "Determination of tensile stress-strain properties of vulcanized rubber or thermoplastic rubber" to test the tensile strength, and record the test results in Table 1, where the greater the tensile strength, the better the tensile properties.
[0065] Table 1 sample <![CDATA[Wear volume / cm 3 > Tensile strength / Mpa Example 1 0.098 13.5 Example 2 0.084 15.2 Example 3 0.084 15.3 Example 4 0.083 15.4 Example 5 0.087 14.7 Example 6 0.086 14.8 Example 7 0.076 15.3 Example 8 0.075 15.4 Example 9 0.074 15.2 Example 10 0.079 15.3 Embodiment 11 0.078 15.1 Example 12 0.067 15.3 Embodiment 13 0.067 15.4 Embodiment 14 0.066 15.2 Embodiment 15 0.069 15.2 Example 16 0.069 15.3 Embodiment 17 0.062 16.3 Embodiment 18 0.062 16.3 Embodiment 19 0.061 16.4 Comparative Example 1 0.138 12.1 Comparative Example 2 0.096 13.9 Data analysis Specifically, in combination with the test results of Examples 2-4 and Example 1, the wear volume of Examples 2-4 is 0.083-0.084 cm 3 , the tensile strength is 15.2-15.4Mpa, and the wear volume of Example 1 is 0.098cm 3 , the tensile strength is 13.5Mpa; the analysis is as follows, the difference between Example 2-4 and Example 1 is that: the friction-increasing filler also contains carbon fiber, on the one hand, the carbon fiber improves the wear resistance of the plastic material, on the other hand, the carbon fiber can play a bridging role, which can increase the effective bonding between silica and polypropylene, thereby improving the tensile properties of the plastic material.
[0066] Specifically, in combination with the test results of Examples 7-9 and Example 4, the wear volume of Examples 7-9 is 0.074-0.076 cm 3 The wear volume of Example 4 is 0.083 cm 3 ; The analysis is as follows. The difference between Examples 7-9 and Example 4 is that dodecyl triethoxysilane improves the surface hydrophobicity of silicon dioxide, reduces the wear on the surface of the plastic material, and effectively improves the wear resistance of the plastic material.
[0067] Specifically, in combination with the test results of Examples 12-14 and Example 9, the wear volume of Examples 12-14 is 0.066-0.067 cm 3 The wear volume of Example 9 is 0.074 cm 3 ; The analysis is as follows. The difference between Examples 12-14 and Example 9 is that polymethyl hydrogen siloxane performs hydrophobic modification on the carbon fiber, thereby improving the hydrophobicity of the carbon fiber, which has a positive effect on improving the wear resistance of the plastic material.
[0068] Specifically, in combination with the test results of Examples 17-19 and Example 14, the wear volume of Examples 17-19 is 0.061-0.062 cm 3 , the tensile strength is 16.3-16.4Mpa, and the abrasion volume of Example 14 is 0.066cm 3 , tensile strength is 15.2Mpa; analysis is as follows, the difference between Examples 17-19 and Example 14 is that dodecyl dimethyl benzyl ammonium chloride is also added to the plastic material. On the one hand, dodecyl dimethyl benzyl ammonium chloride can enhance the adsorption effect between modified silica and modified carbon fiber, and on the other hand, dodecyl dimethyl benzyl ammonium chloride can reduce the surface tension of the plastic material matrix, thereby having a positive effect on improving the wear resistance and tensile properties of the plastic material.
[0069] Specifically, based on the test results of Example 1 and Comparative Example 1, the wear volume of Example 1 is 0.098 cm 3 , the tensile strength is 13.5Mpa, and the wear volume of comparative example 1 is 0.138cm 3 , the tensile strength is 12.1Mpa; the analysis is as follows, the difference between Example 1 and Comparative Example 1 is that: a friction-increasing filler prepared from silicon dioxide is added to the plastic material, thereby effectively improving the wear resistance and tensile properties of the plastic material.
[0070] Specifically, based on the test results of Example 4 and Comparative Example 2, the wear volume of Example 4 is 0.083 cm 3 , the tensile strength is 15.4Mpa, and the wear volume of comparative example 2 is 0.096cm 3, the tensile strength is 13.9Mpa; the analysis is as follows, the difference between Example 4 and Comparative Example 2 is that: a friction-increasing filler prepared by mixing carbon fiber and silica is added to the plastic material, thereby effectively improving the wear resistance and tensile properties of the plastic material.
[0071] The above are all preferred embodiments of the present application, and the protection scope of the present application is not limited thereto. Therefore, any equivalent changes made according to the structure, shape, and principle of the present application should be included in the protection scope of the present application.
Claims
1. A wear-resistant plastic material, characterized in that: The invention comprises the following raw materials in parts by weight: 100-120 parts of polypropylene, 5-10 parts of friction-increasing filler, 1-3 parts of polyol ester and 1-3 parts of calcium stearate; the friction-increasing filler comprises silicon dioxide.
2. The wear-resistant plastic material according to claim 1, characterized in that: The friction-increasing filler also includes carbon fiber.
3. A wear-resistant plastic material according to claim 2, characterized in that: The mass ratio of the silicon dioxide to the carbon fiber is 1:(3.12-3.34).
4. The wear-resistant plastic material according to claim 2, characterized in that: The modified preparation method of silicon dioxide comprises the following steps: Add silicon dioxide to anhydrous ethanol, stir evenly, then add deionized water and ammonia water, stir again, add dodecyltriethoxysilane, heat to react, wash and dry in sequence after the reaction is completed to obtain modified silicon dioxide.
5. The wear-resistant plastic material according to claim 4, characterized in that: The mass ratio of silicon dioxide to dodecyltriethoxysilane is 1: (0.6-0.8) The wear-resistant plastic material according to claim 4 is characterized in that: the modification preparation method of the carbon fiber comprises the following steps: The carbon fiber, polymethylhydrogensiloxane and deionized water are mixed and then subjected to homogeneous reaction. After the reaction is complete, the mixture is cooled to room temperature, and then filtered and dried in sequence to obtain the modified carbon fiber.
6. The wear-resistant plastic material according to claim 6, characterized in that: The mass ratio of the carbon fiber to polymethyl hydrogen siloxane is 1:(0.2-0.4).
7. The wear-resistant plastic material according to claim 6, characterized in that: Also included is 1-3 parts of dodecyldimethylbenzyl ammonium chloride.
8. A method for preparing the wear-resistant plastic material as claimed in claim 1, comprising the following steps: After the polypropylene and the friction-increasing filler are mixed evenly, the polyol ester and calcium stearate are added and mixed evenly again to obtain a mixture; the mixture is then extruded and formed, and finally the extrudate is cooled, pelletized and packaged in sequence to obtain a plastic material.