Core-shell nanocomposite as well as preparation method and application thereof

By forming a nano-silica fiber layer on the surface of the polytetrafluoroethylene emulsion and forming a core-shell nanocomposite material, the problem of poor wear resistance of polytetrafluoroethylene is solved, and its self-lubricating and adsorption properties is improved, which is suitable for industrial applications. .

CN118931083APending Publication Date: 2024-11-12LANZHOU INSTITUTE OF CHEMICAL PHYSICS CHINESE ACADEMY OF SCIENCES +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410917659.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-10
Publication Date
2024-11-12

Smart Images

  • Figure CN118931083A_ABST
    Figure CN118931083A_ABST
Patent Text Reader

Abstract

The invention provides a core-shell nano composite material as well as a preparation method and application thereof, and belongs to the technical field of polymer nano materials. The invention provides a core-shell nano composite material. The core-shell nano composite material comprises a polytetrafluoroethylene-based inner-layer core-shell emulsion polymer and a nano silicon dioxide fiber layer coating the surface of the polytetrafluoroethylene-based inner-layer core-shell emulsion polymer, the polytetrafluoroethylene-based inner layer core-shell emulsion polymer comprises a core body and a shell; the core body is a polytetrafluoroethylene emulsion, and the shell is a copolymer of an acryloyl-containing monomer and an alkoxy silane monomer containing double bonds; the nano silicon dioxide fiber layer is of a mesoporous structure and is composed of a plurality of radial nano silicon dioxide fibers. The core-shell nano composite material provided by the invention does not damage chemical bonds and chemical structures of polytetrafluoroethylene, has excellent self-lubricating performance and adsorption performance, and also has excellent wear resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymer nanomaterials, and specifically relates to a core-shell nanocomposite material and a preparation method and application thereof. Background Art

[0002] Polytetrafluoroethylene (PTFE) and its composite materials are widely used in aerospace and mechanical motion parts. It is a lubricating material with excellent corrosion resistance, good thermal stability and low friction coefficient. Although it has excellent lubricity, it has poor wear resistance and is difficult to meet the needs of harsh working conditions, so it needs to be chemically modified.

[0003] Since the surface of polytetrafluoroethylene is chemically inert, it is difficult to chemically modify the surface. Studies have reported on improving the surface activity of polytetrafluoroethylene by light radiation and plasma treatment. Chinese patent CN202210970641.4 uses infrared laser to irradiate the surface of polytetrafluoroethylene to obtain a high roughness and high oxidation degree surface; Chinese patent CN201610055057.0 uses a plasma treatment surface method, and grafts acrylic acid on its surface. After cold pressing and heat treatment, an α-manganese dioxide-graphene-polytetrafluoroethylene wear-resistant and friction-reducing composite material is prepared. However, after irradiation and plasma treatment, the chemical bonds (CF bonds) of polytetrafluoroethylene will be destroyed, which will affect its self-lubricating properties. Summary of the invention

[0004] In view of this, the object of the present invention is to provide a core-shell nanocomposite material and its preparation method and application. The core-shell nanocomposite material provided by the present invention does not destroy the chemical bonds and chemical structure of polytetrafluoroethylene, has excellent self-lubricating and adsorption properties, and also has excellent wear resistance.

[0005] In order to achieve the above object, the present invention provides the following scheme:

[0006] The present invention provides a core-shell nanocomposite material, comprising a polytetrafluoroethylene-based inner core-shell emulsion polymer and a nano-silicon dioxide fiber layer coated on the surface of the polytetrafluoroethylene-based inner core-shell emulsion polymer;

[0007] The polytetrafluoroethylene inner core-shell emulsion polymer comprises a core and an outer shell; the core is a polytetrafluoroethylene emulsion, and the outer shell is a copolymer containing an acryl monomer and an alkoxysilane monomer containing a double bond;

[0008] The nano silicon dioxide fiber layer has a mesoporous structure and is composed of a plurality of radial nano silicon dioxide fibers.

[0009] Preferably, the mass ratio of the polytetrafluoroethylene based inner core-shell emulsion polymer to the nano-silica fiber layer is (3-6):(8-12); the mass ratio of the polytetrafluoroethylene emulsion to the copolymer is (5-8):(3-6).

[0010] Preferably, the core-shell nanocomposite material has a particle size of 400 to 800 nm and a specific surface area of ​​100 to 600 m 2 / g, pore volume is 0.2~1cm 3 / g, pore size is 2~12nm.

[0011] The present invention provides a method for preparing the core-shell nanocomposite material described in the above scheme, comprising the following steps:

[0012] In an inert atmosphere, a polytetrafluoroethylene emulsion, an acryl-containing monomer, an alkoxysilane monomer containing a double bond, first water, an aqueous solution of a first initiator, and an aqueous solution of a second initiator are first mixed and copolymerized to obtain a polytetrafluoroethylene-based inner core-shell emulsion polymer;

[0013] The alkaline catalyst, the cationic surfactant, the co-surfactant, the second water and the polytetrafluoroethylene-based inner core-shell emulsion polymer are mixed for a second time to obtain an aqueous phase mixed solution;

[0014] performing a third mixing of the silicon source and the organic solvent to obtain an oil phase;

[0015] The oil phase and the water phase mixed solution are fourthly mixed to perform a hydrolysis condensation reaction to form a nano silicon dioxide fiber layer on the surface of the polytetrafluoroethylene-based inner core-shell emulsion polymer to obtain the core-shell nanocomposite material.

[0016] Preferably, the acryl-containing monomer includes one or more of methacrylic acid, methyl methacrylate, α-methacrylic acid, butyl acrylate and acrylic acid; the double bond-containing alkoxysilane monomer includes one or more of 3-(isomethacryloyloxy)propyltrimethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, allyltrimethoxysilane and acetoxypropyltrimethoxysilane.

[0017] Preferably, the copolymerization reaction temperature is 70-80° C. and the reaction time is 4 hours.

[0018] Preferably, the silicon source comprises orthosilicate; and the mass ratio of the silicon source to the organic solvent is (1-70):(30-200).

[0019] Preferably, the temperature of the hydrolysis condensation reaction is 60 to 130° C., and the time is 12 to 24 hours.

[0020] The present invention provides the application of the core-shell nanocomposite material described in the above scheme or the core-shell nanocomposite material prepared by the preparation method described in the above scheme in the field of lubrication.

[0021] Preferably, the application method comprises: using the core-shell nanocomposite material as a liquid lubricant adsorbent or as a lubricant material additive.

[0022] The present invention provides a core-shell nanocomposite material, comprising a polytetrafluoroethylene-based inner core-shell emulsion polymer and a nano-silica fiber layer coated on the surface of the polytetrafluoroethylene-based inner core-shell emulsion polymer; the polytetrafluoroethylene-based inner core-shell emulsion polymer comprises a core body and an outer shell; the core body is a polytetrafluoroethylene emulsion, and the outer shell is a copolymer containing an acryl monomer and an alkoxysilane monomer containing a double bond; the nano-silica fiber layer is a mesoporous structure, and is composed of a number of radial nano-silica fibers. The core-shell nanocomposite material provided by the present invention has the advantages of soft and hard phases (PTFE as a core soft phase, and a nano-silica fiber layer as a hard phase), and does not destroy the chemical structure and chemical bonds (CF bonds) of polytetrafluoroethylene, and is coated to avoid the phase separation problem and dispersibility problem caused by physically mixing soft and hard phases, and at the same time makes it have excellent self-lubricating properties. The core-shell nanocomposite material provided by the present invention has uniform particle size, large specific surface area, controllable pore size, and good adsorption of liquid lubricants.

[0023] The core-shell particles (core-shell nanocomposite materials) provided by the present invention have both the excellent lubrication performance of polytetrafluoroethylene and the dendritic silica shell that plays the role of a rolling bearing, and have excellent wear resistance. The two have an excellent synergistic lubrication mechanism. When subjected to pressure extrusion during the friction process, the core-shell structure changes from a rolling spherical structure to an ellipsoidal structure, and eventually leaks out the polytetrafluoroethylene core to form a uniform phase. Since the core-shell particles are connected by chemical bonding, and the core-shell particles have good adsorption to the surface of the friction substrate, a uniform transfer film is formed on the substrate and the friction pair surface.

[0024] The present invention provides a method for preparing the core-shell nanocomposite material described in the above scheme. The present invention uses a polytetrafluoroethylene emulsion as a core through simple chemical bonding, and without destroying its chemical structure, coats a layer of nano-silica fiber layer on its surface. The nano-silica fiber layer has a mesoporous structure and is composed of a plurality of radial nano-silica fibers, which is similar to a hierarchical dendritic structure. A new core-shell material with excellent pore size and specific surface area is prepared, which has broad application prospects in adsorption, corrosion resistance and self-lubrication.

[0025] The preparation method provided by the invention is simple to operate, has low raw material cost, is environmentally friendly, has a wide range of applications, has potential application prospects, and is suitable for industrial mass production. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0027] Figure 1 TEM images of different materials in Example 1, wherein (a) is a TEM image of PTFE, (b) is a TEM image of a PTFE@polymer copolymer core-shell composite material, (c) is a TEM image of a PTFE@DFNS core-shell nanocomposite material, and (d) is an enlarged TEM image of a PTFE@DFNS core-shell nanocomposite material;

[0028] Figure 2 TEM mapping image of the PTFE@DFNS core-shell nanocomposite prepared in Example 1;

[0029] Figure 3 The infrared spectra of the PTFE@polymer copolymer core-shell composite material and the PTFE@DFNS core-shell nanocomposite material of Example 1 are shown;

[0030] Figure 4 Thermogravimetric curves of the PTFE@DFNS core-shell nanocomposite prepared in Example 1, and the PTFE@DFNS@ILs-1 and PTFE@DFNS@ILs-2 prepared in Application Examples 1 to 2;

[0031] Figure 5 The friction curves of different samples under 0.1Hz and 3N conditions;

[0032] Figure 6 This is the TEM image of the core-shell nanocomposite material prepared in Example 2. DETAILED DESCRIPTION

[0033] The present invention provides a core-shell nanocomposite material, comprising a polytetrafluoroethylene-based inner core-shell emulsion polymer and a nano-silicon dioxide fiber layer coated on the surface of the polytetrafluoroethylene-based inner core-shell emulsion polymer; the polytetrafluoroethylene-based inner core-shell emulsion polymer comprises a core body and an outer shell; the core body is a polytetrafluoroethylene emulsion, and the outer shell is a copolymer containing an acryl monomer and an alkoxysilane monomer containing a double bond;

[0034] The nano silicon dioxide fiber layer has a mesoporous structure and is composed of a plurality of radial nano silicon dioxide fibers.

[0035] In the present invention, the mass ratio of the polytetrafluoroethylene based inner core-shell emulsion polymer and the nano-silica fiber layer is preferably (3-6):(8-12), and more preferably (3.5-5.5):(9-11); the mass ratio of the polytetrafluoroethylene emulsion and the copolymer is preferably (5-8):(3-6), and more preferably (5.5-7.5):(3.5-5.5).

[0036] In the present invention, the particle size of the core-shell nanocomposite material is preferably 400-800 nm, and the specific surface area is preferably 100-600 m 2 / g, and the pore volume is preferably 0.2 to 1 cm 3 / g, and the pore size is preferably 2 to 12 nm.

[0037] In the present invention, the dendritic silica with mesoporous structure has a central radial dendritic structure with a hierarchical pore structure, has a larger specific surface area than traditional mesoporous materials, and thus has higher pore permeability, pore volume and adsorption capacity; has abundant pores, making its surface easy to chemically modify, and has good affinity with other materials and strong ability to load guest substances, so that it can adsorb liquid lubricants at a high content. It also has excellent chemical stability, biocompatibility, corrosion resistance and ultraviolet absorbability. The present invention compounds it with polytetrafluoroethylene, does not destroy the chemical bonds and chemical structure of polytetrafluoroethylene, and can make the composite material have excellent self-lubricating properties and adsorption properties, and at the same time has excellent wear resistance.

[0038] The core-shell nanocomposite material provided by the present invention has the advantages of soft and hard phases, and does not destroy the chemical structure and chemical bonds (CF bonds) of polytetrafluoroethylene, and is coated to avoid the phase separation problem and dispersibility problem caused by physical mixing of soft and hard phases, and at the same time has excellent self-lubricating properties. The core-shell nanocomposite material provided by the present invention has uniform particle size, large specific surface area, controllable pore size, and good adsorption of liquid lubricants.

[0039] The core-shell particles (core-shell nanocomposite materials) provided by the present invention have both the excellent lubrication performance of polytetrafluoroethylene and the dendritic silica shell that plays the role of a rolling bearing, and have excellent wear resistance. The two have an excellent synergistic lubrication mechanism. When subjected to pressure extrusion during the friction process, the core-shell structure changes from a rolling spherical structure to an ellipsoidal structure, and eventually leaks out the polytetrafluoroethylene core to form a uniform phase. Since the core-shell particles are connected by chemical bonding, and the core-shell particles have good adsorption to the surface of the friction substrate, a uniform transfer film is formed on the substrate and the friction pair surface.

[0040] The present invention provides a method for preparing the core-shell nanocomposite material described in the above scheme, comprising the following steps:

[0041] In an inert atmosphere, a polytetrafluoroethylene emulsion, an acryl-containing monomer, an alkoxysilane monomer containing a double bond, first water, an aqueous solution of a first initiator, and an aqueous solution of a second initiator are first mixed and copolymerized to obtain a polytetrafluoroethylene-based inner core-shell emulsion polymer;

[0042] A solution of an alkaline catalyst, a cationic surfactant, a co-surfactant, a second water and the polytetrafluoroethylene-based inner core-shell emulsion polymer are mixed for a second time to obtain an aqueous phase mixed solution;

[0043] performing a third mixing of the silicon source and the organic solvent to obtain an oil phase;

[0044] The oil phase and the water phase mixed solution are fourthly mixed to perform a hydrolysis condensation reaction to form a nano silicon dioxide fiber layer on the surface of the polytetrafluoroethylene-based inner core-shell emulsion polymer to obtain the core-shell nanocomposite material.

[0045] Unless otherwise specified, the materials and equipment used in the present invention are all commercially available products.

[0046] The invention first mixes polytetrafluoroethylene emulsion, acryl-containing monomer, double-bond-containing alkoxysilane monomer, first water, aqueous solution of a first initiator and aqueous solution of a second initiator under an inert atmosphere, and performs polymerization reaction to obtain a polytetrafluoroethylene inner layer core-shell emulsion polymer.

[0047] In the present invention, the solid content of the polytetrafluoroethylene emulsion is preferably 30% to 70%, and more preferably 50% to 60%.

[0048] In the present invention, the acryl-containing monomer preferably includes one or more of methacrylic acid, methyl methacrylate, α-methacrylic acid, butyl acrylate and acrylic acid; the double bond-containing alkoxysilane monomer preferably includes one or more of 3-(isomethacryloyloxy)propyltrimethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, allyltrimethoxysilane and acetoxypropyltrimethoxysilane.

[0049] In the present invention, the first initiator and the second initiator are independently preferably one or more of potassium persulfate, ammonium persulfate, azobisisobutylnitrile, azobisisobutylimidazole hydrochloride, benzoyl, hydrogen peroxide, diisophenyl peroxide, di-tert-butyl peroxide, ferrous sulfate and sodium sulfite.

[0050] In the present invention, the mass ratio of the polytetrafluoroethylene emulsion and the acryl-containing monomer is preferably (20-100): (70-200), more preferably (50-90): (80-150), and more preferably (60-80): (90-120); the mass ratio of the polytetrafluoroethylene emulsion and the double-bond-containing alkoxysilane monomer is preferably (20-100): (20-120), more preferably (50-90): (30-85), and more preferably (60-80): (40-70); the mass ratio of the polytetrafluoroethylene emulsion and the first initiator is preferably (20-100): (0.3-1.5), and more preferably (50-90): (0.5 ~1.2), more preferably (60~80):(0.7~1.1); the mass ratio of the polytetrafluoroethylene emulsion to the second initiator is preferably (20~100):(0.2~0.8), further preferably (50~90):(0.3~0.8), more preferably (60~80):(0.4~0.6); the mass ratio of the polytetrafluoroethylene emulsion to the total water for copolymerization (including the water in the aqueous solution of the first initiator and the water in the aqueous solution of the second initiator and the first water) is preferably (20~100):(800~1800), more preferably (60~80):(800~1200), more preferably (50~90):(900~1100).

[0051] In the present invention, the first mixing preferably includes mixing the polytetrafluoroethylene emulsion and the first water, then adding the acryl-containing monomer for a first stirring, then adding the first initiator aqueous solution for a second stirring, and finally adding the second initiator aqueous solution simultaneously.

[0052] In the present invention, the temperature of the first mixing is preferably 70 to 80°C, and more preferably 72 to 78°C.

[0053] In the present invention, the mixing of the polytetrafluoroethylene emulsion and water is preferably carried out under ultrasonic conditions; the ultrasonic time is preferably 10 to 50 minutes.

[0054] In the present invention, the first stirring time is preferably 3 to 6 hours, more preferably 4 to 5.5 hours; the second stirring time is preferably 4 to 6 hours, more preferably 4.5 to 5.5 hours.

[0055] In the present invention, the speeds of the first stirring and the second stirring are independently preferably 300 to 450 rpm, and more preferably 320 to 420 rpm.

[0056] After the second stirring is completed, the present invention preferably adds a pH adjuster to adjust the pH value of the obtained mixed emulsion to neutral.

[0057] The present invention has no special requirements on the type and amount of the pH adjuster. It is sufficient to use a reagent well known in the art to adjust the pH value of the obtained mixed emulsion to neutral.

[0058] In the present invention, when the acryl-containing monomer has an ester group, it will partially decompose during the heating process, or when the acryl-containing monomer contains a carboxyl group to make the reaction system weakly acidic, in order to make the polymerization conditions of the double-bond alkoxysilane monomer consistent with the aforementioned reaction conditions and avoid affecting the progress of the reaction, the pH value of the solution should be adjusted to neutral.

[0059] In the present invention, the acrylic group-containing monomer is preferably added by dropwise addition; the dropwise addition speed is preferably 20 s / drop.

[0060] In the present invention, the concentration of the aqueous solution of the first initiator is preferably 0.1wt.% to 0.8wt.%, more preferably 0.15wt.% to 0.4wt.%; the aqueous solution of the first initiator is preferably added by dropwise addition; the dropwise addition speed is preferably 10 to 20 s / drop, more preferably 12 to 17 s / drop.

[0061] In the present invention, the double bond-containing alkoxysilane monomer is preferably added by dropwise addition; the dropwise addition speed is preferably 10 to 15 s / drop, and more preferably 12 to 14 s / drop.

[0062] In the present invention, the concentration of the aqueous solution of the second initiator is preferably 0.1wt.% to 0.4wt.%, more preferably 0.15wt.% to 0.4wt.%; the aqueous solution of the second initiator is preferably added by dropwise addition; the dropwise addition speed is preferably 10 to 20 s / drop, more preferably 12 to 17 s / drop.

[0063] In the present invention, the copolymerization reaction temperature is preferably 70 to 80° C., more preferably 72 to 78° C.; the copolymerization reaction time is preferably 4 hours.

[0064] In the present invention, the copolymerization reaction is preferably carried out under stirring conditions; the stirring speed is preferably 300 to 450 rpm, and more preferably 320 to 420 rpm.

[0065] After the copolymerization reaction is completed, the present invention preferably cools the obtained reaction solution to room temperature, then removes the unreacted monomers and emulsifier by centrifugal washing with ethanol, and then disperses the obtained polytetrafluoroethylene-based inner core-shell emulsion polymer in ethanol for standby use.

[0066] In the present invention, polytetrafluoroethylene emulsion is used as the core, and acryl-containing monomers and double-bond-containing alkoxysilane monomers are coated on the outer layer of the polytetrafluoroethylene emulsion through emulsion copolymerization, thereby forming a polytetrafluoroethylene-based inner layer core-shell emulsion polymerization product, and the surface of the core-shell structure contains a large number of alkoxy groups, which can provide a large number of active sites for coating a new silica shell layer.

[0067] After obtaining the polytetrafluoroethylene-based inner core-shell emulsion polymer, the present invention performs a second mixing of the alkaline catalyst, the cationic surfactant, the cosurfactant, the second water and the polytetrafluoroethylene-based inner core-shell emulsion polymer to obtain an aqueous phase mixed solution.

[0068] In the present invention, the alkaline catalyst preferably includes one or more of urea, ethanolamine, sodium hydroxide and ethylenediamine.

[0069] In the present invention, the cationic surfactant preferably includes cetyltrimethylammonium bromide and / or cetyltrimethylammonium chloride.

[0070] In the present invention, the co-surfactant preferably includes one or more of ethanol, propanol, butanol, isopropanol and pentanol.

[0071] In the present invention, the mass ratio of the copolymerization product (i.e., the polytetrafluoroethylene-based inner core-shell emulsion polymer after ethanol dispersion) to the alkaline catalyst is preferably (10-400):(5-360), further preferably (50-300):(10-250), and more preferably (100-250):(10-180); the mass ratio of the alkaline catalyst to the cationic surfactant is preferably (5-360):(10-80), further preferably (10-250):(20-60), and more preferably (10-180):(30-55); the mass ratio of the alkaline catalyst to the co-surfactant is preferably (5-360):(10-120), further preferably (10-250):(60-100), and more preferably (10-180):(60-90).

[0072] In the present invention, before the second mixing, the polytetrafluoroethylene-based inner core-shell emulsion polymer dispersed in ethanol is preferably subjected to ultrasound; the ultrasound time is preferably 20 minutes.

[0073] In the present invention, the second mixing preferably includes: dissolving the alkaline catalyst in the second water to obtain a solution of the alkaline catalyst; mixing the ultrasonically dispersed polytetrafluoroethylene-based inner core-shell emulsion polymer and the solution of the alkaline catalyst, and then sequentially adding a cationic surfactant and a co-surfactant.

[0074] In the present invention, the molar concentration of the alkaline catalyst solution is preferably 0.2 to 10 mol / L, and more preferably 0.4 to 5 mol / L.

[0075] In the present invention, the second mixing time is preferably 15 minutes; the second mixing time is preferably calculated from the completion of the addition of the alkaline catalyst.

[0076] In the present invention, the second mixing is preferably performed under the condition of mechanical stirring; the rate of the mechanical stirring is preferably 200 to 1200 rpm, and more preferably 500 to 800 rpm.

[0077] In the present invention, the co-surfactant is preferably added in a dropwise manner, and the addition speed is preferably 2s / drop.

[0078] In the present invention, the silicon source and the organic solvent are mixed for the third time to obtain an oil phase.

[0079] In the present invention, the silicon source preferably includes orthosilicate, and the orthosilicate preferably includes one or more of tetraethyl orthosilicate, tetrabutyl orthosilicate and methyl orthosilicate; the organic solvent preferably includes one or more of n-hexane, cyclohexane, decalin, toluene and p-diphenylene; the mass ratio of the silicon source to the organic solvent is preferably (1-70):(30-200), further preferably (5-50):(40-150), more preferably (8-20):(40-150); in the present invention, the mass ratio of the silicon source to the alkaline catalyst is preferably (1-70):(1-36), more preferably (8-20):(1-18).

[0080] After completing the third mixing, the present invention preferably allows the obtained oil phase to stand; the standing time is preferably 5 minutes.

[0081] After obtaining the oil phase and the water phase mixed solution, the present invention fourthly mixes the oil phase and the water phase mixed solution to perform a hydrolysis condensation reaction to form a nano silicon dioxide fiber layer on the surface of the polytetrafluoroethylene-based inner core-shell emulsion polymer to obtain the core-shell nanocomposite material.

[0082] In the present invention, the fourth mixing preferably includes: adding the oil phase into the aqueous phase mixed solution.

[0083] In the present invention, the temperature of the hydrolysis condensation reaction is preferably 60 to 130° C., more preferably 65 to 110° C., and more preferably 70 to 90° C.; the time of the hydrolysis condensation reaction is preferably 12 to 24 h, and more preferably 15 to 20 h.

[0084] In the present invention, the heating rate to the hydrolysis condensation reaction temperature is preferably 5 to 20° C. / min, more preferably 8 to 15° C. / min, and more preferably 10° C. / min.

[0085] In the process of the hydrolysis condensation reaction of the present invention, the silicon source is hydrolyzed into oligomers, and then the oligomers are polymerized into silicon dioxide.

[0086] After the hydrolysis condensation reaction is completed, the present invention preferably performs post-treatment on the obtained reaction emulsion, and the post-treatment preferably comprises the following steps:

[0087] The obtained reaction emulsion was cooled to room temperature and subjected to the first centrifugal washing: the reaction emulsion was subjected to the first centrifugal washing three times with anhydrous ethanol and deionized water respectively, the first centrifugal speed was 8500 rpm, the time was 3 min, and the unreacted silicon source and other emulsions were removed;

[0088] The product after centrifugal washing is dispersed in ethanol and then hydrochloric acid is added to form an acid solution mixed with hydrochloric acid and ethanol, hot solvent extraction is performed, anhydrous ethanol and deionized water are used for second centrifugal washing three times in sequence, and then drying is performed to obtain the core-shell nanocomposite material.

[0089] In the present invention, the concentration of the hydrochloric acid is preferably 1 mol / L; the volume ratio of the hydrochloric acid to ethanol is preferably (3-6):150.

[0090] In the present invention, the temperature of the hot solvent extraction is preferably 60-80°C, more preferably 75°C, the time is preferably 10-24h, more preferably 15h; the hot solvent extraction is preferably carried out under stirring; the stirring rate is preferably 600-700rpm.

[0091] The present invention preferably uses a mixed hot solvent of hydrochloric acid and ethanol to extract twice to completely remove the cationic surfactant.

[0092] In the present invention, the speed of the second centrifugal washing is preferably 4000-10000 rpm, and more preferably 9000 rpm; the second centrifugal washing is preferably performed until the solution is neutral.

[0093] In the present invention, the drying is preferably freeze drying; the freeze drying temperature is preferably -70°C, and the time is preferably 24 to 40 hours.

[0094] The invention can effectively remove impurities in the hydrolysis and polycondensation reaction product and blockages in the pores of silicon dioxide by adopting centrifugal washing and drying to obtain powder with sparse and loose particles.

[0095] The invention adopts a double-continuous phase microemulsion method to carry out a hydrolysis-condensation reaction. In the double-phase reaction, microemulsion droplets coated with polytetrafluoroethylene are formed, and the microemulsion droplets serve as nanoreactors for the growth of dendritic silica shells. The hydrolysis-condensation reaction is carried out to obtain a dendritic silica core-shell nanocomposite material; and the core-shell material coats the polytetrafluoroethylene without destroying its chemical structure.

[0096] In the present invention, the core-shell nanocomposite material exists in the form of powder particles at room temperature. The particles are spherical, and partial adhesion between particles is allowed. However, the particles are uniformly dispersed in acetone or ethanol solutions.

[0097] The invention can adjust the pore size, specific surface area and fiber layer thickness of the core-shell nano composite material by changing the ratio of the reactant oil phase, the water phase and the surfactant.

[0098] The present invention provides the application of the core-shell nanocomposite material described in the above scheme or the core-shell nanocomposite material prepared by the preparation method described in the above scheme in the field of lubrication.

[0099] In the present invention, the application method preferably comprises: using the core-shell nanocomposite material as a liquid lubricant adsorbent or as a lubricant material additive.

[0100] When the core-shell nanocomposite material is used as a liquid lubricant adsorbent, the step of applying preferably comprises:

[0101] The core-shell nanocomposite material and a liquid lubricant are mixed and vacuum wet impregnated to obtain a core-shell nanocomposite material containing oil.

[0102] In the present invention, the liquid lubricant preferably includes one or more of imidazole type ionic liquid, polyolefin lubricating oil and liquid paraffin; in the present invention, the imidazole type ionic liquid preferably includes C 8 H 15 PF 6 N 2 or C 8 H 15 BF 4 N 2 The mass content of the liquid lubricant in the core-shell nanocomposite material is preferably 10 to 45%, and more preferably 15 to 35%.

[0103] The present invention uses a mesoporous dendritic silica core-shell nanocomposite material as an adsorbent, absorbs a liquid lubricant through vacuum impregnation, and combines the dendritic silica wall of the outer shell of the core-shell nanocomposite material with the liquid lubricant through hydrogen bonds and van der Waals forces to prepare a mesoporous dendritic silica core-shell nanocomposite material containing a liquid lubricant.

[0104] When the core-shell nanocomposite material is used as a lubricant additive, the present invention has no special requirements on the application steps, and steps well known in the art can be used.

[0105] In the present invention, the lubricating material preferably includes a polymer self-lubricating material, such as one or more of polyimide, polyamide and polymer coating lubricating materials. In the embodiment of the present invention, it is specifically an epoxy resin coating.

[0106] In order to further illustrate the present invention, a core-shell nanocomposite material provided by the present invention and its preparation method and application are described in detail below in conjunction with the accompanying drawings and examples, but they should not be construed as limiting the scope of protection of the present invention.

[0107] Example 1

[0108] The preparation method of the core-shell nanocomposite material comprises the following steps:

[0109] Preparation of polytetrafluoroethylene-based inner core-shell emulsion polymer: First, a precursor polymer emulsion is prepared by emulsion copolymerization: 8g polytetrafluoroethylene (PTFE) emulsion and 110g deionized water are added to a five-necked flask, and then ultrasonically dispersed for 15 minutes to mix them evenly. Under condenser reflux and nitrogen protection, the reaction is carried out by heating in an oil bath, and the resulting dispersion is heated to 75°C and stirred for 20 minutes, then 10g methyl methacrylate solution is slowly dripped into the flask and reacted at a constant temperature for 4 hours, and then 30g of an initiator potassium persulfate aqueous solution (mass concentration is 0.3wt.%) is slowly dripped, and the addition speed is 15s / drop, and the dripping is completed in about 4 hours. After 2 hours of isothermal reaction, the pH value of the obtained reaction emulsion was adjusted to neutral using diluted ammonia water; at the same time, 5g of 3-(isobutylene acyloxy)propyltrimethoxysilane solution and 10g of initiator potassium persulfate aqueous solution (mass concentration of 0.4wt.%) were slowly dripped into the flask at a rate of 15s / drop, and the dripping was completed in about 2 hours. After 4 hours of isothermal reaction, the sample was cooled to room temperature. Unreacted monomers and emulsifiers were removed by centrifugal washing with ethanol, and then dispersed in ethanol to prepare a 250mL solution, i.e., a polytetrafluoroethylene-based inner core-shell emulsion polymer, recorded as PTFE@polymer copolymer.

[0110] Preparation of core-shell nanocomposite materials: The polytetrafluoroethylene-based inner core-shell emulsion polymer was ultrasonicated for 20 minutes, and then 8 g was taken out and added to a three-necked flask, and mechanically stirred at a speed of 300 rpm at room temperature, and then 50 g of urea aqueous solution (2 mol / L) and 3 g of cationic surfactant hexadecyltrimethylammonium bromide were added and mixed evenly in the three-necked flask. Then 6 g of co-surfactant n-butanol (added in a dropwise manner at a rate of 2 s / drop) was slowly added to further stabilize the emulsion, and mixed and stirred for 15 minutes to obtain an aqueous phase mixed solution.

[0111] 12 g of tetraethyl orthosilicate and 60 g of cyclohexane were mixed evenly in a beaker and allowed to stand for 5 min to obtain an oil phase;

[0112] Then slowly and evenly add the oil phase to the above-mentioned three-necked flask containing the aqueous phase mixed solution, add it within 45min, and the stirring speed during the addition process is maintained at 300rpm. After the addition is completed, constant temperature (room temperature) continues to stir for 30min. Afterwards, the stirring speed is adjusted to 600rpm, the reaction emulsion is heated to 75°C, and a hydrolysis condensation reaction is carried out, and the constant temperature reaction is 20h. After the reaction is completed, the obtained reaction emulsion is cooled to room temperature and centrifuged and washed. The reaction emulsion is centrifuged and washed three times with anhydrous ethanol and deionized water respectively, and the centrifugal rate is 8500rpm, and the time is 3min. Then dispersed in 150mL ethanol, a core-shell nanocomposite ethanol solution with a cationic surfactant is obtained.

[0113] The cationic surfactant was removed by hot solvent extraction: the obtained core-shell nanocomposite ethanol solution with cationic surfactant was added to a three-necked flask, 5 mL of 1 mol / L hydrochloric acid was added, the solution temperature was raised to 70°C, the heating rate was 10°C / min, and the magnetic stirring speed was 650 rpm, and the stirring was continued for 12 hours. The operation was carried out under sealed conditions. After the solvent extraction reaction was completed, the solution was cooled to room temperature and then centrifuged and washed. The obtained reaction product was centrifuged and washed three times with anhydrous ethanol and deionized water, respectively, at a centrifugal speed of 8000 rpm for 3 minutes, until the solution was neutral. The extraction operation was repeated twice. Finally, the sample was freeze-dried at -70°C for 36 hours to obtain a core-shell nanocomposite powder, which was recorded as PTFE@DFNS.

[0114] Example 2

[0115] The preparation method of the core-shell nanocomposite material comprises the following steps:

[0116] The preparation steps of the polytetrafluoroethylene-based inner core-shell emulsion polymer are the same as those in Example 1 and are denoted as PTFE@polymer copolymer.

[0117] Emulsion polymerization of dendritic silica core-shell composite material: The prepared polytetrafluoroethylene-based inner core-shell emulsion polymer was ultrasonicated for 20 minutes, and then 25g was taken out and added to a three-necked flask and mechanically stirred at 300rpm at room temperature. Then 60g of urea aqueous solution (2mol / L) and 3g of cationic surfactant hexadecyltrimethylammonium bromide were mixed evenly in a three-necked flask. Then 8g of co-surfactant n-butanol was slowly added (added in a dropwise manner at a rate of 2s / drop) to further stabilize the emulsion, and mixed and stirred for 15min to obtain an aqueous phase mixed solution.

[0118] 15 g of ethyl orthosilicate and 60 g of cyclohexane were mixed evenly in a beaker and allowed to stand for 5 min to obtain an oil phase;

[0119] Then slowly and evenly add the oil phase to the three-necked flask containing the aqueous phase mixed solution, add it within 45min, and keep the stirring speed at 300rpm during the addition. After the addition is completed, keep stirring at constant temperature (room temperature) for 30min. Afterwards, the stirring speed is adjusted to 600rpm, the reactant emulsion is heated to 75°C, and a hydrolysis condensation reaction is carried out, and the constant temperature reaction is carried out for 20h. After the reaction is completed, the obtained reaction emulsion is cooled to room temperature. Then centrifugal washing is carried out, and the reaction emulsion is centrifuged and washed three times with anhydrous ethanol and deionized water respectively, and the centrifugal rate is 8500rpm, and the time is 3min. Then dispersed in 150mL ethanol, a core-shell nanocomposite ethanol solution with a cationic surfactant is obtained.

[0120] The cationic surfactant was removed by hot solvent extraction: the obtained core-shell nanocomposite ethanol solution with cationic surfactant was added to a three-necked flask, 5 mL of 1 mol / L hydrochloric acid was added, the solution temperature was raised to 70°C, the heating rate was 10°C / min, and the magnetic stirring speed was 650 rpm, and the stirring was continued for 12 hours. The operation was carried out under sealed conditions. After the solvent extraction reaction was completed, the solution was cooled to room temperature and then centrifuged and washed. The obtained reaction product was centrifuged and washed three times with anhydrous ethanol and deionized water, respectively, at a centrifugal speed of 8000 rpm for 3 minutes, until the solution was neutral. The extraction operation was repeated twice. Finally, the sample was freeze-dried at -70°C for 36 hours to obtain a core-shell nanocomposite powder, which was recorded as PTFE@DFNS.

[0121] Example 3

[0122] The preparation method of the core-shell nanocomposite material comprises the following steps:

[0123] Preparation of polytetrafluoroethylene-based inner core-shell emulsion polymer: First, prepare the precursor polymer emulsion by emulsion copolymerization: add 8g polytetrafluoroethylene (PTFE) emulsion and 110g deionized water into a five-necked flask, and then ultrasonically disperse for 15min to mix them evenly. Under the reflux of the condenser and the protection of nitrogen, the reaction is carried out by heating in an oil bath, and the resulting dispersion is heated to 75°C and stirred for 20min, then 10g methacrylic acid solution is slowly dripped into the flask and reacted at a constant temperature for 4h, and then 30g of initiator ammonium persulfate aqueous solution (mass concentration is 0.3wt.%) is slowly dripped, and the addition rate is 15s / drop, and it drips in about 4h. After isothermal reaction for 2h, the pH of the reacted emulsion is adjusted to neutral with diluted ammonia water; at the same time, 5g acetoxypropyl trimethoxysilane solution and 10g of initiator potassium persulfate aqueous solution (mass concentration is 0.4wt.%) are slowly dripped into the flask, and the addition rate is 15s / drop, and it drips in about 2h. After 4 h of isothermal reaction, the sample was cooled to room temperature and obtained by centrifugal washing with ethanol to remove unreacted monomers and emulsifiers, and then dispersed in ethanol to prepare a 250 mL solution, namely, a polytetrafluoroethylene-based inner core-shell emulsion polymer, recorded as PTFE@polymer copolymer.

[0124] Preparation of core-shell nanocomposite materials: The polytetrafluoroethylene-based inner core-shell emulsion polymer was ultrasonicated for 20 minutes, and then 15 g was taken out and added to a three-necked flask, and mechanically stirred at a speed of 300 rpm at room temperature, and then a mixed aqueous solution of 1:1 with a mass ratio of urea solution and sodium hydroxide solution (both with a concentration of 0.4 mol / L) was added, and the mass of the mixed aqueous solution was 50 g, and 4 g of cationic surfactant hexadecyltrimethylammonium chloride was mixed evenly in a three-necked flask. Then 6 g of co-surfactant n-pentanol (added in a dropwise manner at a rate of 2 s / drop) was slowly added to further stabilize the emulsion, and mixed and stirred for 15 minutes to obtain an aqueous phase mixed solution.

[0125] 15 g of methyl orthosilicate and 60 g of cyclohexane were mixed evenly in a beaker and allowed to stand for 5 min to obtain an oil phase;

[0126] Then slowly and evenly add the oil phase to the three-necked flask containing the aqueous phase mixed solution, add it within 45min, and keep the stirring speed at 300rpm during the addition. After the addition is completed, keep stirring at constant temperature (room temperature) for 30min. Afterwards, the stirring speed is adjusted to 600rpm, the reactant emulsion is heated to 75°C, and a hydrolysis condensation reaction is carried out, and the constant temperature reaction is carried out for 20h. After the reaction is completed, the obtained reaction emulsion is cooled to room temperature. Then centrifugal washing is carried out, and the reaction emulsion is centrifuged and washed three times with anhydrous ethanol and deionized water respectively, and the centrifugal rate is 8500rpm, and the time is 3min. Then dispersed in 150mL ethanol, a core-shell nanocomposite ethanol solution with a cationic surfactant is obtained.

[0127] Removal of cationic surfactant by hot solvent extraction: Add the obtained core-shell nanocomposite ethanol solution with cationic surfactant into a three-necked flask, then add 5mL of 1mol / L hydrochloric acid, raise the solution temperature to 70℃, and the heating rate is 10℃ / min. Stir continuously for 12h at a magnetic stirring speed of 650rpm. This operation is carried out under sealed conditions. After the solvent extraction reaction is completed, the solution is cooled to room temperature and then centrifuged and washed. The reaction product is centrifuged three times with anhydrous ethanol and deionized water, respectively, at a centrifugal speed of 8000rpm for 3min, until the solution is neutral. Repeat the extraction operation twice. Finally, the sample is freeze-dried at -70℃ for 36h to obtain a core-shell nanocomposite powder, which is recorded as PTFE@DFNS.

[0128] Example 4

[0129] The preparation method of the core-shell nanocomposite material comprises the following steps:

[0130] Preparation of polytetrafluoroethylene-based inner core-shell emulsion polymer: First, prepare the precursor polymer emulsion. Use emulsion copolymerization: add 10g polytetrafluoroethylene (PTFE) emulsion and 110g deionized water into a five-necked flask, and then ultrasonically disperse for 15 minutes to mix them evenly. Under condenser reflux and nitrogen protection, heat the reaction in an oil bath, heat the resulting dispersion to 75°C and stir for 20 minutes, then slowly drip 10g of α-methylacrylic acid solution into the flask and react at a constant temperature for 4 hours, then slowly drip 30g of initiator sodium sulfite aqueous solution (mass concentration is 0.3wt.%), the addition rate is 15s / drop, and the dripping is completed in about 4 hours. After 2 hours of isothermal reaction, the pH of the reacted emulsion was adjusted to neutral using diluted ammonia water; at the same time, 5g of acetoxypropyltrimethoxysilane solution and 10g of initiator sodium sulfite aqueous solution (mass concentration of 0.4wt.%) were slowly dripped into the flask at a rate of 15s / drop, and the dripping was completed in about 2 hours. After 4 hours of isothermal reaction, the sample was cooled to room temperature. Unreacted monomers and emulsifiers were removed by centrifugal washing with ethanol, and then dispersed in ethanol to prepare a 250mL solution, i.e., a polytetrafluoroethylene-based inner core-shell emulsion polymer, recorded as PTFE@polymer copolymer.

[0131] Preparation of core-shell nanocomposite materials: The prepared polytetrafluoroethylene-based inner core-shell emulsion polymer was ultrasonicated for 20 minutes, and then 20g was taken out and added to a three-necked flask for mechanical stirring at a speed of 300rpm at room temperature. Then, a mixed aqueous solution of 1:1 mass ratio of the prepared urea solution and ethanolamine solution (both at a concentration of 2 mol / L) was prepared, and the mass of the mixed aqueous solution was 60g. 3g of the cationic surfactant hexadecyltrimethylammonium bromide was mixed evenly in a three-necked flask. Then 6g of the co-surfactant n-pentanol (added in a dropwise manner at a rate of 2s / drop) was slowly added to further stabilize the emulsion, and mixed and stirred for 15min to obtain an aqueous phase mixed solution.

[0132] 15 g of butyl orthosilicate and 60 g of decalin were mixed evenly in a beaker and allowed to stand for 5 min to obtain an oil phase;

[0133] Then slowly and evenly add the oil phase to the three-necked flask containing the aqueous phase mixed solution, add it within 45min, and keep the stirring speed at 300rpm during the addition. After the addition is completed, keep stirring at constant temperature (room temperature) for 30min. Then adjust the stirring speed to 600rpm, heat the reactant emulsion to 75℃, carry out hydrolysis condensation reaction, and react at constant temperature for 20h. After the reaction is completed, cool the obtained reaction emulsion to room temperature. Then centrifuge and wash, and centrifuge the reaction emulsion with anhydrous ethanol and deionized water three times, respectively, at a centrifugal rate of 8500rpm for 3min. Then disperse in 150mL ethanol to obtain a core-shell nanocomposite ethanol solution with a cationic surfactant.

[0134] The cationic surfactant was removed by hot solvent extraction: the obtained core-shell nanocomposite ethanol solution with cationic surfactant was added to a three-necked flask, and then 5 mL of 1 mol / L hydrochloric acid was added, and the solution temperature was raised to 70°C at a heating rate of 10°C / min. The solution was stirred for 12 hours at a magnetic stirring speed of 650 rpm. The operation was carried out under sealed conditions. After the solvent extraction reaction was completed, the solution was cooled to room temperature and then centrifuged. The reaction product was centrifuged three times with anhydrous ethanol and deionized water, respectively, at a centrifugal speed of 8000 rpm for 3 minutes until the solution was neutral. The extraction operation was repeated twice. Finally, the sample was vacuum dried at 70°C for 20 hours to obtain a core-shell nanocomposite powder, which was recorded as PTFE@DFNS.

[0135] Example 5

[0136] The preparation method of the core-shell nanocomposite material comprises the following steps:

[0137] Preparation of polytetrafluoroethylene-based inner core-shell emulsion polymer: First, prepare the precursor polymer emulsion. Use emulsion copolymerization: add 10g polytetrafluoroethylene (PTFE) emulsion and 110g deionized water into a five-necked flask, and then ultrasonically disperse for 15min to mix them evenly. Under the reflux of the condenser and the protection of nitrogen, the reaction is carried out by heating in an oil bath, and the resulting dispersion is heated to 75°C and stirred for 20min. After that, 10g butyl acrylate solution is slowly dripped into the flask and reacted at a constant temperature for 4h, and then 30g of initiator potassium sulfite aqueous solution (mass concentration is 0.3wt.%) is slowly dripped, and the addition rate is 15s / drop, and it drips in about 4h. After isothermal reaction for 2h, the pH of the reacted emulsion is adjusted to neutral using diluted ammonia water. Then 5g of vinyl trimethoxysilane solution and 10g of initiator sodium sulfite aqueous solution (mass concentration is 0.4wt.%) are slowly dripped into the flask at the same time, and the addition rate is 15s / drop, and it drips in about 2h. After 4 h of isothermal reaction, the sample was cooled to room temperature and obtained by centrifugal washing with ethanol to remove unreacted monomers and emulsifiers, and then dispersed in ethanol to prepare a 250 mL solution, namely, a polytetrafluoroethylene-based inner core-shell emulsion polymer, recorded as PTFE@polymer copolymer.

[0138] Preparation of core-shell nanocomposite materials: The prepared polytetrafluoroethylene-based inner core-shell emulsion polymer was ultrasonicated for 20 minutes, and then 20g was taken out and added to a three-necked flask for mechanical stirring at 300rpm at room temperature. Then, a mixed aqueous solution of 1:1 of ethylenediamine solution and ethanolamine solution (both at a concentration of 3 mol / L) was prepared, and the mass of the mixed aqueous solution was 60g. 3g of cationic surfactant hexadecyltrimethylammonium chloride was mixed evenly in a three-necked flask. Then 6g of co-surfactant propanol was slowly added (added in a dropwise manner at a rate of 2s / drop) to further stabilize the emulsion, and mixed and stirred for 15min to obtain an aqueous phase mixed solution.

[0139] 15 g of butyl orthosilicate and 80 g of decalin were mixed evenly in a beaker and allowed to stand for 5 min to obtain an oil phase;

[0140] Then slowly and evenly add the oil phase to the three-necked flask containing the aqueous phase mixed solution, add it within 45 minutes, and keep the stirring speed at 300rpm during the addition. After the addition is completed, keep stirring at constant temperature (room temperature) for 30 minutes. After that, adjust the stirring speed to 600rpm, heat the reaction emulsion to 75°C, carry out hydrolysis condensation reaction, and react at constant temperature for 20 hours. After the reaction is completed, cool the resulting solution to room temperature. Then centrifuge and wash, and centrifuge the reaction emulsion with anhydrous ethanol and deionized water for three times, respectively, at a centrifugal rate of 8500rpm for 3 minutes. Then disperse in 150mL ethanol to obtain an ethanol solution of a core-shell nanocomposite material with a cationic surfactant.

[0141] The cationic surfactant was removed by hot solvent extraction: the obtained core-shell nanocomposite ethanol solution with cationic surfactant was added to a three-necked flask, and then 5 mL of 1 mol / L hydrochloric acid was added, and the solution temperature was raised to 70°C at a heating rate of 10°C / min. The solution was stirred for 12 hours at a magnetic stirring speed of 650 rpm. The operation was carried out under sealed conditions. After the solvent extraction reaction was completed, the solution was cooled to room temperature and then centrifuged. The reaction product was centrifuged three times with anhydrous ethanol and deionized water, respectively, at a centrifugal speed of 8000 rpm for 3 minutes until the solution was neutral. The extraction operation was repeated twice. Finally, the sample was vacuum dried at 70°C for 20 hours to obtain a core-shell nanocomposite powder, which was recorded as PTFE@DFNS.

[0142] Application Examples 1-2

[0143] Application of PTFE@DFNS core-shell nanocomposites in adsorption of liquid lubricants:

[0144] 0.5 g of the PTFE@DFNS core-shell nanocomposite obtained in Example 1 was placed in a sand core filter device, and an organic filter membrane was used to adsorb the liquid lubricant by vacuum wet impregnation. The vacuum degree of the vacuum pump was -0.082 MPa. The liquid lubricants were 5 mL of imidazole lubricant C 8 H 15 PF 6 N 2 and C 8 H 15 BF 4 N 2The immersion time was 15 min, and the adsorption was repeated three times. Then, the samples were centrifuged and washed twice with deionized water at a centrifugal speed of 5500 rpm for 3 min to remove the liquid lubricant blocked in the pores. Finally, the samples were vacuum dried at 80 °C for 20 h to obtain dendritic silica oil-containing lubricating materials, which were recorded as PTFE@DFNS@ILs-1 and PTFE@DFNS@ILs-2, respectively.

[0145] Structure and performance testing

[0146] Figure 1 It is the TEM image of different materials in Example 1, wherein (a) is the TEM image of PTFE, (b) is the TEM image of PTFE@polymer copolymer core-shell composite material, (c) is the TEM image of PTFE@DFNS core-shell nanocomposite material, and (d) is the TEM enlarged image of PTFE@DFNS core-shell nanocomposite material (wherein, DFNS represents silica shell). It can be seen from (a) that the PTFE micromorphology is an ellipse of a long strip; it can be seen from (b) that the PTFE@polymer copolymer core-shell composite material has an obvious core-shell structure, and the particles are obviously bonded to each other, and the PTFE of the kernel has changed from an ellipse to a circular structure. It can be seen from (c) that the TEM morphology image of the PTFE@DFNS core-shell nanocomposite material has an obvious core-shell structure, and the dendritic nano-silica shell has an obvious fiber layer dendritic structure. (d) is a local enlarged image of (c), and it can be clearly seen from the figure that the dendritic silica shell is more obvious. And the dendritic layered structure has a large density and a compact structure, and the structure has excellent specific surface area and pore size.

[0147] Figure 2 The distribution diagram of the element surface scan of the PTFE@DFNS core-shell nanocomposite obtained in Example 1 shows the distribution of C, O, F, and Si elements. It can be seen from the figure that for the characteristic elements of PTFE, the F element is mainly distributed inside, which corresponds to PTFE as the core. And the silicon element is mainly distributed outside, and the dendritic silica is mainly distributed in the shell, which corresponds to the element distribution. These all illustrate the synthesis of the dendritic silica core-shell nanocomposite with a mesoporous structure.

[0148] Figure 3 The infrared spectra of the PTFE@polymer copolymer core-shell composite material (i.e., the PTFE@polymer copolymer core-shell nanocomposite material in the figure) and the PTFE@DFNS core-shell nanocomposite material prepared in Example 1 are shown in FIG. Figure 3 It can be seen that the PTFE@polymer copolymer core-shell composite material is at 1233.25 cm -1 and 1158.06cm -1The peaks are the asymmetric stretching vibration and symmetric stretching vibration of the CF bond, and the peaks are weak, which indicates that the polymer copolymer is coated on PTFE. For the PTFE@DFNS core-shell nanocomposite at 1099.31cm -1 and 3444.06cm -1 There are obvious broad and strong absorption peaks, which belong to the asymmetric stretching vibrations of Si-O-Si and Si-OH, respectively, indicating that there are a large number of hydroxyl groups on the surface of PTFE@DFNS, and the surface activity of PTFE after dendritic silica coating is significantly improved, and PTFE@DFNS is successfully prepared.

[0149] Figure 4 The thermogravimetric curves of the PTFE@DFNS core-shell nanocomposite prepared in Example 1 and the PTFE@DFNS@ILs-1 and PTFE@DFNS@ILs-2 prepared in Application Examples 1 to 2 are shown in FIG. Figure 4 It can be seen that PTFE@DFNS adsorbs C 8 H 15 PF 6 N 2 The content of PTFE@DFNS is 30.1%, and the ionic liquid C 8 H 15 BF 4 N 2 The content is 27.5%.

[0150] Figure 5 The friction curves of different samples (the samples are: pure epoxy resin coating, epoxy resin coating with 3wt.% added PTFE@DFNS and epoxy resin coating with 3wt.% added PTFE@DFNS@ILs, and the preparation method can be a method known in the art) under 0.1Hz, 3N conditions are shown in Table 1. The friction coefficient and volume wear rate of different samples are shown in Table 2.

[0151] from Figure 5 It can be seen from Table 1 that under normal friction, compared with the pure epoxy resin coating (denoted as PureEP), the epoxy resin coating with 3wt.% addition of PTFE@DFNS (denoted as PTFE@DFNS-EP) and the epoxy resin coating with PTFE@DFNS@ILs-1 (denoted as PTFE@DFNS@ILs-EP) prepared under the same conditions showed that Figure 5It can be concluded from Table 1 that the dendritic silica core-shell nanocomposites with mesoporous structures have excellent tribological properties. In particular, the epoxy resin coating of the PTFE@DFNS@ILs nanocomposite has the lowest friction coefficient and volume wear rate, which further illustrates that PTFE@DFNS@ILs has good self-lubricating properties and excellent wear resistance.

[0152] Table 1 Friction coefficient and volume wear rate of different samples (nanomaterial addition amount is 3wt.%)

[0153]

[0154]

[0155] Figure 6 TEM image of the dendritic silica core-shell nanocomposite (PTFE@DFNS) prepared in Example 2. Figure 6 It can be seen that the nanoparticles have an obvious core-shell structure, and the polytetrafluoroethylene inside presents a round structure, which is very different from the polytetrafluoroethylene emulsion. The particles are uniform and have a mesoporous structure on the surface.

[0156] The performance test results of the dendritic silica core-shell nanocomposites prepared in Examples 2 to 5 are similar to those in Example 1.

[0157] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. People can also obtain other embodiments based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.

Claims

1. A core-shell nanocomposite material, characterized in that: It comprises a polytetrafluoroethylene-based inner core-shell emulsion polymer and a nano-silicon dioxide fiber layer coated on the surface of the polytetrafluoroethylene-based inner core-shell emulsion polymer; The polytetrafluoroethylene inner core-shell emulsion polymer comprises a core and an outer shell; the core is a polytetrafluoroethylene emulsion, and the outer shell is a copolymer containing an acryl monomer and an alkoxysilane monomer containing a double bond; The nano silicon dioxide fiber layer has a mesoporous structure and is composed of a plurality of radial nano silicon dioxide fibers.

2. The core-shell nanocomposite material according to claim 1, characterized in that: The mass ratio of the polytetrafluoroethylene inner core-shell emulsion polymer to the nano-silica fiber layer is (3-6):(8-12); the mass ratio of the polytetrafluoroethylene emulsion to the copolymer is (5-8):(3-6).

3. The core-shell nanocomposite material according to claim 1 or 2, characterized in that: The core-shell nanocomposite material has a particle size of 400 to 800 nm and a specific surface area of ​​100 to 600 m 2 / g, pore volume is 0.2~1cm 3 / g, pore size is 2~12nm.

4. The method for preparing the core-shell nanocomposite material according to any one of claims 1 to 3, characterized in that: The following steps are involved: In an inert atmosphere, a polytetrafluoroethylene emulsion, an acryl-containing monomer, an alkoxysilane monomer containing a double bond, first water, an aqueous solution of a first initiator, and an aqueous solution of a second initiator are first mixed and copolymerized to obtain a polytetrafluoroethylene-based inner core-shell emulsion polymer; The alkaline catalyst, the cationic surfactant, the co-surfactant, the second water and the polytetrafluoroethylene-based inner core-shell emulsion polymer are mixed for a second time to obtain an aqueous phase mixed solution; performing a third mixing of the silicon source and the organic solvent to obtain an oil phase; The oil phase and the water phase mixed solution are fourthly mixed to perform a hydrolysis condensation reaction to form a nano silicon dioxide fiber layer on the surface of the polytetrafluoroethylene-based inner core-shell emulsion polymer to obtain the core-shell nanocomposite material.

5. The preparation method according to claim 4, characterized in that: The acryl-containing monomer includes one or more of methacrylic acid, methyl methacrylate, α-methacrylic acid, butyl acrylate and acrylic acid; the double-bond-containing alkoxysilane monomer includes one or more of 3-(isomethacryloyloxy)propyltrimethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, allyltrimethoxysilane and acetoxypropyltrimethoxysilane.

6. The preparation method according to claim 4 or 5, characterized in that: The copolymerization reaction temperature is 70-80° C. and the reaction time is 4 hours.

7. The preparation method according to claim 4, characterized in that: The silicon source includes orthosilicate; the mass ratio of the silicon source to the organic solvent is (1-70):(30-200).

8. The preparation method according to claim 4, characterized in that: The temperature of the hydrolysis condensation reaction is 60-130° C. and the time is 12-24 hours.

9. Use of the core-shell nanocomposite material according to claims 1 to 3 or the core-shell nanocomposite material prepared by the preparation method according to any one of claims 4 to 8 in the field of lubrication.

10. The use according to claim 9, characterized in that: The application method comprises: using the core-shell nanocomposite material as a liquid lubricant adsorbent or as a lubricant material additive.

Citation Information

Patent Citations

  • Polytetrafluoroethylene-based core-shell type mesoporous composite material, preparation method thereof, oil-immersed mesoporous composite material and application

    CN112961536A

  • Dendritic silicon dioxide oil-containing material as well as preparation method and application thereof

    CN117987191A

  • Preparation method for polysiloxane-acrylate / styrene copolymer with large particle size and core-shell structure

    WO2018192222A1