High-thermal-conductivity and high-insulation electronic packaging material with pearl layer structure and preparation method and application thereof

By modifying graphene with organic polyamines and polyphenols and constructing a nacre structure through a high-temperature molding process, the problem of graphene's easy agglomeration in the polymer matrix was solved, resulting in an electronic packaging material with high thermal conductivity and high insulation, thus improving the balance between thermal conductivity and insulation performance.

CN118931110APending Publication Date: 2024-11-12AKM ELECTRONICS INDAL PANYU
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411162444.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing polymer-based electronic packaging materials have poor thermal conductivity, and graphene tends to agglomerate in the matrix resin and its electrical conductivity does not meet the requirements for insulation performance, making it difficult to achieve a balance between high thermal conductivity and high insulation performance.

Method used

Graphene was modified with organic polyamines and organic polyphenols, and a high thermal conductivity and high insulation electronic packaging material with a nacre structure was constructed through a high-temperature molding process. This improved the dispersibility of graphene in the resin and formed a continuous thermally conductive network.

Benefits of technology

The orderly arrangement of graphene in the resin matrix was achieved, which improved the thermal conductivity of the material while maintaining high insulation and adhesion, thus extending its service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118931110A_ABST
    Figure CN118931110A_ABST
Patent Text Reader

Abstract

The invention relates to a high-thermal-conductivity and high-insulation electronic packaging material with a pearl layer structure and a preparation method and application thereof. The preparation method comprises the following steps: modifying graphene by adopting organic polyamine and organic polyphenol; uniformly mixing the obtained modified graphene, epoxy resin, a curing agent and a solvent, pre-curing and volatilizing the solvent, and then preparing the packaging material through a high-temperature mold process. The modified graphene is modified by the organic matter, the modification method is simple and convenient, the dispersity problem of the modified graphene is solved, the conductivity of the modified graphene is weakened, the performance balance of high heat conductivity and high insulation is achieved, and the high-heat-conductivity and high-insulation electronic packaging material of a pearl layer structure is constructed by a high-temperature mold pressing process aiming at a two-dimensional sheet-shaped graphene structure. The heat-conducting property of the composite material is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of microelectronic packaging materials, and in particular relates to a nacreous structured high thermal conductivity and high insulation electronic packaging material, and a preparation method and application thereof. Background Art

[0002] As the application of 5G and 6G technologies becomes more and more widespread, electronic devices are also developing towards high frequency, high speed, integration and miniaturization, which puts forward higher and more diversified requirements for the thermal conductivity, insulation, high reliability and other properties of electronic packaging materials. Thermal conduction, that is, heat transfer, is an energy transfer phenomenon caused by temperature difference. There are three basic modes: heat conduction, heat convection and heat radiation.

[0003] Traditional electronic packaging materials include glass, ceramics and polymers, among which polymer-based electronic packaging materials occupy about 90% of the market share due to their low cost and easy processing. Pure polymers have excellent insulation properties, but their thermal conductivity is very poor, generally at 0.2 to 0.3 W / mK, so they need to be modified to improve their thermal conductivity.

[0004] Among them, the preparation of thermally conductive particle-filled thermally conductive composite materials is the simplest and most direct method. Graphene has excellent thermal conductivity (5300W / mK), however, under the combined effect of high surface energy and van der Waals force, graphene is prone to serious agglomeration, resulting in poor compatibility with the matrix resin. In addition, the high conductivity of graphene does not meet the requirements of the insulation performance of packaging materials, so it needs to be modified before it can be used in packaging materials.

[0005] Chinese patent document CN 115322521 A provides a method for preparing a high thermal conductivity 3-3 type graphene / epoxy resin composite material, in which nano-scale graphene is assembled into a macro-scale graphene aerogel, the structure and thermal conductivity of the graphene are restored by high-temperature reduction treatment, and then epoxy resin is filled into the three-dimensionally connected graphene aerogel to form a three-dimensional graphene thermal conductive path in the epoxy resin matrix, thereby greatly improving the thermal conductivity of the graphene / epoxy resin composite material at a lower graphene filling amount. The method is relatively complicated. Summary of the invention

[0006] In view of the above problems existing in the prior art, the present invention aims to provide a nacreous structured high thermal conductivity and high insulation electronic packaging material and a preparation method and application thereof.

[0007] The present invention adopts the following technical solution:

[0008] In a first aspect of the present invention, a method for preparing a nacreous structured high thermal conductivity and high insulation electronic packaging material is provided, comprising the steps of:

[0009] (1) mixing an organic polyamine, an organic polyphenol, graphene and deionized water uniformly, reacting at 80 to 100° C. for 8 to 12 hours, and finally removing water by freeze drying or vacuum drying to obtain modified graphene;

[0010] (2) After the modified graphene, epoxy resin, curing agent and solvent obtained in step (1) are uniformly mixed, the solvent is pre-cured to volatilize, and then the nacreous layer structure with high thermal conductivity and high insulation electronic packaging material is prepared through a high-temperature mold process.

[0011] Furthermore, in step (1), the mass ratio of graphene, organic polyphenol and organic polyamine is 1:(0.5-1.0):(0.1-0.5).

[0012] The organic polyamine may be at least one or more of bio-based polyamines, aliphatic polyamines and aromatic polyamines; the organic polyphenol may be at least one or more of tannic acid, dopamine, gallic acid and catechol.

[0013] Furthermore, in step (2), the epoxy resin is at least one or more of bisphenol A epoxy resin, bisphenol F epoxy resin, polypropylene epoxy resin, biphenyl epoxy resin, vinyl fluoride epoxy resin, alicyclic ethoxy resin and epoxy resin containing an inorganic skeleton structure.

[0014] Furthermore, in step (2), the curing agent is at least one or more of a phenolic epoxy resin curing agent, an acid anhydride curing agent, a polyamine curing agent and a polyamide curing agent.

[0015] Furthermore, in step (2), the solvent is at least one or more of acetone, butanone, toluene, dichloromethane, N,N-dimethylformamide and N,N-dimethylacetamide.

[0016] Furthermore, in step (2), the amount of modified graphene used is 10-50wt% of the total solid content.

[0017] Furthermore, in step (2), the molar ratio of epoxy groups in the epoxy resin to the curing groups in the curing agent is 1:0.5 to 1.2.

[0018] Furthermore, in step (2), the pre-curing temperature is 60-90°C, and the pre-curing time is 0.5-1h; the high-temperature molding process is pre-pressing at 150-180°C and 3-5MPa for 0.2-0.5h, and then heating to 180-250°C and 5-20MPa for hot pressing for 1-2h.

[0019] The second aspect of the present invention also provides a nacreous structured high thermal conductivity and high insulation electronic packaging material obtained by the preparation method.

[0020] The third aspect of the present invention also provides the application of the high thermal conductivity and high insulation electronic packaging material with the nacre structure in the field of microelectronic packaging materials.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] The present invention adopts organic matter to modify the graphene, and the modification method is simple, which not only solves the problem of its dispersibility, but also weakens its electrical conductivity, thereby achieving a performance balance of high thermal conductivity and high insulation. Furthermore, the distribution state of the two-dimensional flaky graphene material inside the matrix resin affects the performance of the composite material. For the two-dimensional flaky graphene structure, a high thermal conductivity and high insulation electronic packaging material with a pearl layer structure is constructed by a high-temperature molding process suitable for industrialization, thereby providing the thermal conductivity of the composite material. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is a morphological picture of the internal structure of the composite material of Example 1 of the present invention. DETAILED DESCRIPTION

[0024] In order to facilitate the understanding of the present invention, the present invention will be described more fully below with reference to the relevant drawings and embodiments. Preferred embodiments of the present invention are given in the embodiments. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.

[0025] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.

[0026] The reagents used in the following examples, unless otherwise specified, are all commercially available; the methods used in the following examples, unless otherwise specified, are all conventional methods that can be achieved.

[0027] The preparation method of the modified graphene used in the embodiment of the present invention is as follows:

[0028] 2.5 g of graphene, 2.0 g of tannic acid and 0.5 g of diethylenetriamine were added to 30 mL of deionized water, stirred and reacted at 80° C. for 8 h, and then freeze-dried to remove water to obtain organic-coated modified graphene.

[0029] Example 1

[0030] 100g E44, 20g phenolic modified amine curing agent, 12g modified graphene and 50g acetone solvent were selected and uniformly dispersed by mechanical stirring, followed by pre-curing at 60°C for 0.5h to volatilize the acetone solvent, and then pre-pressed at 160°C and 3MPa for 0.5h, heated to 180°C and hot pressed at 10MPa for 1h, and naturally cooled to room temperature to obtain a nacreous structured high thermal conductivity and high insulation electronic packaging material.

[0031] Figure 1 This is a picture of the internal structure of the packaging material obtained in the example. It can be seen that the graphene is orderly arranged inside the resin matrix, forming a continuous heat-conducting network structure similar to pearl layer.

[0032] Example 2

[0033] 100g E44, 20g phenolic modified amine curing agent, 24g modified graphene and 60g acetone solvent were selected and evenly dispersed by mechanical stirring, followed by pre-curing at 60°C for 0.5h to volatilize the acetone solvent, and then pre-pressed at 160°C and 3MPa for 0.5h, heated to 180°C and hot pressed at 10MPa for 1h, and naturally cooled to room temperature to obtain a nacreous structured high thermal conductivity and high insulation electronic packaging material.

[0034] Example 3

[0035] 100g E44, 20g phenolic modified amine curing agent, 36g modified graphene and 60g acetone solvent were selected and uniformly dispersed by mechanical stirring, followed by pre-curing at 60°C for 0.5h to volatilize the acetone solvent, and then pre-pressed at 160°C and 3MPa for 0.5h, heated to 180°C and hot pressed at 10MPa for 1h, and naturally cooled to room temperature to obtain a nacreous structured high thermal conductivity and high insulation electronic packaging material.

[0036] Example 4

[0037] 100g E44, 20g phenolic modified amine curing agent, 48g modified graphene and 70g acetone solvent were selected and evenly dispersed by mechanical stirring, followed by pre-curing at 60°C for 0.5h to volatilize the acetone solvent, and then pre-pressed at 160°C and 3MPa for 0.5h, heated to 180°C and hot pressed at 10MPa for 1h, and naturally cooled to room temperature to obtain a nacreous structured high thermal conductivity and high insulation electronic packaging material.

[0038] Example 5

[0039] 100g E44, 20g phenolic modified amine curing agent, 60g modified graphene and 80g acetone solvent were selected and uniformly dispersed by mechanical stirring, followed by pre-curing at 60°C for 0.5h to volatilize the acetone solvent, and then pre-pressed at 160°C and 3MPa for 0.5h, heated to 180°C and hot pressed at 10MPa for 1h, and naturally cooled to room temperature to obtain a nacreous structured high thermal conductivity and high insulation electronic packaging material.

[0040] Comparative Examples 1-5

[0041] Control samples 1-5 were prepared by hot pressing using unmodified graphene and the processes corresponding to implementations 1-5.

[0042] Comparative Example 6

[0043] 100g E44, 20g phenolic modified amine curing agent and 20g acetone solvent were selected and evenly dispersed by mechanical stirring, followed by pre-curing at 60°C for 0.5h to volatilize the acetone solvent, and then pre-pressed at 160°C and 3MPa for 0.5h, heated to 180°C and 10MPa for hot pressing for 1h, and naturally cooled to a pure resin-based high thermal conductivity and high insulation electronic packaging material.

[0044] Performance Test:

[0045] Thermal conductivity: The thermal diffusion coefficient α of the implementation case and the comparison case was tested using the LFA467 laser scattering thermal conductivity instrument of the German NETZSCH company, m2 / s. The volume density ρ of the material was tested using the drainage method and an electronic balance, g / cm3. According to the formula

[0046] λ=α×ρ×Cp

[0047] Calculate the thermal conductivity λ of the composite material, W / (m·K).

[0048] Dielectric strength: The insulation strength of the implementation case and the comparison case was tested using Taiwan Chroma 19073.

[0049] Glass transition temperature: The glass transition temperature of the polymer was measured using a differential scanning calorimeter (DSC 214, NETZSCH, Germany). The temperature was rapidly raised to 200°C at a rate of 10°C / min in a nitrogen environment, balanced for 5 minutes to eliminate the thermal history, then dropped to -50°C at a rate of 10°C / min, and then raised to 200°C at a rate of 10°C / min again. The glass transition temperature was obtained from the second heating curve.

[0050] Adhesion test: Copper foil was selected as the substrate, and the adhesion of the sample was tested using the UTM 5000 universal testing machine produced by Shenzhen Sansi Company.

[0051] Table 1 Comparison of composite material properties between the embodiment and the comparative example

[0052]

[0053] According to the test results of comparative example 6, the thermal conductivity of pure epoxy resin E44 is only 0.2W / mK. From the test results in Table 1, it can be seen that the filling of graphene thermal conductive particles increases the thermal conductivity of the composite material, especially the graphene particles modified by organic polyamines and organic polyphenols in the present invention. The thermal conductivity increases with the increase of the filling amount. Since graphene has excellent electrical conductivity, its insulation strength decreases with the increase of the filling amount. There are two reasons for the improvement of thermal conductivity. One is that the modified graphene can be dispersed in the epoxy resin without agglomeration due to intermolecular forces. The other is that the high-temperature molding process promotes its orderly arrangement inside the resin matrix, forming a continuous thermal conductive network structure similar to the pearl layer ( Figure 1 The introduction of organic polyamine and organic polyphenol polar groups also increases the adhesion between the composite material and the copper foil, and will not cause cracking and warping during the use of microelectronic packaging, thus extending its service life.

[0054] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0055] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A method for preparing a pearl layer structured high thermal conductivity and high insulation electronic packaging material, characterized in that: Includes steps: (1) mixing an organic polyamine, an organic polyphenol, graphene and deionized water uniformly, reacting at 80 to 100° C. for 8 to 12 hours, and finally removing water by freeze drying or vacuum drying to obtain modified graphene; (2) After the modified graphene, epoxy resin, curing agent and solvent obtained in step (1) are uniformly mixed, the solvent is pre-cured to volatilize, and then the nacreous layer structure with high thermal conductivity and high insulation electronic packaging material is prepared through a high-temperature mold process.

2. The preparation method according to claim 1, characterized in that: In step (1), the organic polyamine is at least one or more of bio-based polyamines, aliphatic polyamines and aromatic polyamines; the organic polyphenol is at least one or more of tannic acid, dopamine, gallic acid and catechol; and the mass ratio of graphene, organic polyphenol and organic polyamine is 1:(0.5-1.0):(0.1-0.5).

3. The preparation method according to claim 1, characterized in that: In step (2), the epoxy resin is at least one or more of bisphenol A epoxy resin, bisphenol F epoxy resin, polypropylene epoxy resin, biphenyl epoxy resin, vinyl fluoride epoxy resin, alicyclic ethoxy resin and epoxy resin containing an inorganic skeleton structure.

4. The preparation method according to claim 1, characterized in that: In step (2), the curing agent is at least one or more of a phenolic epoxy resin curing agent, an acid anhydride curing agent, a polyamine curing agent and a polyamide curing agent.

5. The preparation method according to claim 1, characterized in that: The solvent in step (2) is at least one or more of acetone, butanone, toluene, dichloromethane, N,N-dimethylformamide and N,N-dimethylacetamide.

6. The preparation method according to claim 1, characterized in that: The amount of modified graphene used in step (2) is 10-50wt% of the total solid content.

7. The preparation method according to claim 1, characterized in that: In step (2), the molar ratio of epoxy groups in the epoxy resin to the curing groups in the curing agent is 1:0.5-1.

2.

8. The preparation method according to claim 1, characterized in that: In step (2), the pre-curing temperature is 60-90°C and the pre-curing time is 0.5-1h; the high temperature molding process is pre-pressing at 150-180°C and 3-5MPa for 0.2-0.5h, then heating to 180-250°C and 5-20MPa for hot pressing for 1-2h.

9. A pearl layer structured high thermal conductivity and high insulation electronic packaging material obtained by the preparation method according to any one of claims 1 to 8.

10. Application of the high thermal conductivity and high insulation electronic packaging material with a pearl layer structure according to claim 9 in the field of microelectronic packaging materials.