High-rigidity nylon composite material and preparation method thereof
By adopting the combination of aliphatic and aromatic nylon with high-content glass fiber in automotive parts and optimizing the treatment in screw extruder, the strength and dispersion of nylon composite materials are solved, and high strength and high temperature resistance are achieved The performance is suitable for the lightweight and energy consumption of automotive parts.
Patent Information
- Application Number
- CN202411174490.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-12
AI Technical Summary
The prior art is difficult to achieve high strength and high temperature resistance in automotive parts, especially in engine parts, and traditional plastic materials are difficult to meet these requirements. At the same time, high-content glass fibers are unevenly dispersed in nylon composite materials, resulting in broken stripping problems. .
The combination of aliphatic nylon and aromatic nylon with high content glass fiber is adopted, and the ZME threaded element is used to blend it in the screw extruder through the side feeding port, controlling the temperature and vacuum degree in the extruder barrel, and optimizing the mold The pore size of the head-well plate is used to improve the dispersion uniformity and strength of the glass fibers.
The high tensile strength, bending strength and bending modulus of nylon composite materials have been improved, the problems of uneven dispersion of glass fibers and broken strips have been solved, and the overall strength performance of the material has been improved.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of nylon composite materials, and in particular to a high-rigidity nylon composite material and a preparation method thereof. Background Art
[0002] With the development of automobile technology, there are requirements for lightweight parts, reducing the weight of parts and reducing automobile energy consumption; but at the same time, the strength performance of parts should not be reduced. In this process, automobile parts materials that replace steel with plastic have emerged to solve the problem of reducing the weight of parts. However, the strength and hardness of plastic materials need to be further improved, especially for automobile parts located in the engine part of the car, which are required to have high strength and high temperature resistance. Traditional plastic materials are difficult to meet this requirement.
[0003] A Chinese patent with patent publication number CN104194328A discloses a high-gloss, high-fluidity, high-content glass fiber reinforced nylon material and a preparation method thereof. It adopts a combination of branched nylon 6 resin and glass fiber to solve the problems of fluidity and glossiness, but does not involve how to better disperse the glass fiber into the nylon to solve the problem of broken strands.
[0004] Therefore, providing a nylon composite material with good dispersibility and high rigidity is the main technical problem that needs to be solved at present. Summary of the invention
[0005] In order to solve the above technical problems, the first aspect of the present invention provides a high-rigidity nylon composite material, whose preparation raw materials include, by weight: 40 to 60 parts of nylon, 40 to 50 parts of glass fiber, and 4.3 to 9.5 parts of additives, and the nylon includes aliphatic nylon and aromatic nylon.
[0006] In one embodiment, the tensile strength of the high-rigidity nylon composite material is greater than 240 MPa when tested according to ISO 527-1-2012, the flexural strength of the high-rigidity nylon composite material is greater than or equal to 320 MPa when tested according to ISO 178-2019, and the flexural modulus of the high-rigidity nylon composite material is greater than 14000 MPa when tested according to ISO 178-2019.
[0007] In one embodiment, the raw materials for its preparation include 40-50 parts of aliphatic nylon and 5-15 parts of aromatic nylon by weight.
[0008] In one embodiment, the aliphatic nylon is selected from a combination of one or more of nylon 66, nylon 6, and nylon 610.
[0009] In one embodiment, the aliphatic nylon is nylon 66.
[0010] In one embodiment, the aromatic nylon is selected from a combination of one or more of nylon 6I / 6T, nylon 6T, nylon 9T, and nylon 10T.
[0011] In one embodiment, the aromatic nylon is nylon 6I / 6T.
[0012] In order to improve the strength performance of nylon composite materials, the inventors found in the experimental process that by using aliphatic nylon and aromatic nylon with high-content glass fiber for cooperation, the aliphatic nylon is nylon 66, the aromatic nylon is nylon 6I / 6T, the diameter of the glass fiber is 1-50μm, and the length of the glass fiber is 1-5mm, especially when the diameter of the glass fiber is 10μm and the length is 3-4.5mm, the nylon composite material obtained by the cooperation has a tensile strength greater than 240MPa when tested according to ISO 527-1-2012, and a flexural strength greater than or equal to 320MPa when tested according to ISO 178-2019, and a flexural modulus greater than 14000MPa when tested according to ISO178-2019. The inventors speculate that the possible reason is that the functional group structure contained in the aromatic nylon can be a certain interval inside the molecular chain segment of the nylon composite material, so that the glass fiber can be better embedded in the gap between the molecular chain segments to form a strong cross structure, so that the strength performance of the nylon composite material is improved.
[0013] In one embodiment, the diameter of the glass fiber is 1 to 50 μm, and the length of the glass fiber is 1 to 5 mm.
[0014] In a preferred embodiment, the diameter of the glass fiber is 5 to 40 μm, and the length of the glass fiber is 2 to 4.5 mm.
[0015] In a preferred embodiment, the length of the glass fiber includes but is not limited to 2 mm, 2.5 mm, 3 mm, 3.5 mm, 4 mm, and 4.5 mm.
[0016] In a more preferred embodiment, the diameter of the glass fiber is 10 μm.
[0017] In a more preferred embodiment, the glass fiber has a diameter of 10 μm and a length of 3-4.5 mm. The commercially available brand is ECS 301HP and the manufacturer is Chongqing International Composite Materials Co., Ltd.
[0018] In one embodiment, the auxiliary agent is selected from a combination of one or more of a lubricant, a dispersant, a light stabilizer, and an antioxidant.
[0019] In one embodiment, the auxiliary agent includes a lubricant, a dispersant, a light stabilizer, and an antioxidant.
[0020] In one embodiment, the raw materials for its preparation include, by weight, 2-4 parts of lubricant, 2-4 parts of dispersant, 0.1-0.5 parts of light stabilizer, and 0.2-1 parts of antioxidant.
[0021] In a preferred embodiment, the raw materials for its preparation include 3 parts of lubricant, 3 parts of dispersant, 0.3 parts of light stabilizer and 0.6 parts of antioxidant, by weight.
[0022] In one embodiment, the model of the lubricant is CYD-816A, and manufacturers that can purchase it include Weihai Chenyuan Molecular New Materials Co., Ltd.
[0023] In one embodiment, the dispersant is of a model HyPer C182, and manufacturers that can purchase it include Wuhan Hyperbranched Resin Technology Co., Ltd.
[0024] In one embodiment, the light stabilizer is Tinuvin 234, which can be purchased from manufacturers including BASF.
[0025] In one embodiment, the antioxidant includes antioxidants 1096 and 168, and the weight ratio of antioxidant 1096 to antioxidant 168 is 1:1.
[0026] The antioxidant 1096 and antioxidant 168 can be purchased from manufacturers including BASF.
[0027] A second aspect of the present invention provides a method for preparing a high-rigidity nylon composite material, comprising the following steps:
[0028] S1. Mixing aliphatic nylon with additives to obtain material a;
[0029] S2. The aromatic nylon is mixed with material a to obtain material b;
[0030] S3. Add material b and glass fiber into a screw extruder respectively for blending and extrusion to obtain a high-rigidity nylon composite material.
[0031] In one embodiment, in S3, material b is added to the screw extruder through the main feeding port of the screw extruder, and the glass fiber is added to the screw extruder through the side feeding port of the screw extruder. After blending, extrusion, belt drawing, cooling, drying, and pelletizing, a high-rigidity nylon composite material is obtained.
[0032] In one embodiment, the screw extruder is a twin-screw extruder.
[0033] In one embodiment, the side feed port uses a ZME threaded element.
[0034] The technical resistance encountered by the inventors during the experiment is that when a high content of glass fiber is added to the screw extruder, the glass fiber will be crushed due to the shearing action of the screw in the screw extruder, which reduces the strength of the nylon composite material, and when the glass fiber is added, the glass fiber will also accumulate and cannot be better dispersed in the nylon; therefore, in order to increase the uniformity of dispersion of the glass fiber in the nylon and reduce the strong shearing action of the twin screw on the glass fiber, the inventors found during the experiment that the use of ZME threaded elements at the side feed port to transport the glass fiber to the inside of the barrel of the screw extruder and contact it with the molten nylon on the twin screw can solve the above-mentioned technical resistance problem. The possible reason is that the use of ZME threaded elements at the side feed port can disperse the glass fiber into the nylon in a flowing state, forming a better dispersion effect and reducing the strong shearing action of the twin screws in the twin screw extruder on the glass fiber.
[0035] In one embodiment, the temperature inside the barrel of the screw extruder during the blending extrusion in S3 is 250-300°C.
[0036] In a preferred embodiment, the temperature inside the barrel of the screw extruder during the blending extrusion in S3 is 275°C.
[0037] In one embodiment, when performing the blending extrusion in S3, the vacuum degree in the barrel of the screw extruder is set to -0.01 to -0.4 MPa.
[0038] In a preferred embodiment, when performing the blending extrusion in S3, the vacuum degree in the barrel of the screw extruder is set to -0.065 MPA.
[0039] In one embodiment, the hole diameter of the die orifice plate of the screw extruder in S3 is 2 to 2.9 mm.
[0040] In one embodiment, the hole diameter of the die orifice plate of the screw extruder in S3 is 2.5 mm.
[0041] The technical resistance encountered by the inventor during the experiment is that when a high content of glass fiber is mixed with nylon to obtain a nylon composite material, the problem of broken strips will occur. In order to solve the problem of broken strips by better dispersing the glass fiber into nylon, the inventor found during the experiment that when 50 parts of glass fiber are combined with 40-50 parts of aliphatic nylon and 5-15 parts of aromatic nylon to form a nylon composite material, the side feed port uses a ZME threaded element, and the aperture of the die orifice plate of the screw extruder is 2-2.9 mm, especially when the aperture of the die orifice plate is 2.5 mm, the above-mentioned technical resistance can be solved. The possible reason is that when the aperture of the die orifice plate of the screw extruder is 2.5 mm, extrusion pressure can be formed at the screw die, residual gas can be discharged, and a certain orientation effect can be formed, so that the glass fiber can be better dispersed into the nylon material, avoiding the problem of broken strips; but when the aperture of the die orifice plate is greater than 2.9 mm, the problem of broken strips will occur during the processing, and the strength performance of the nylon composite material will be reduced.
[0042] In one embodiment, the head temperature of the screw extruder in S3 is 260-270°C.
[0043] In a preferred embodiment, the head temperature of the screw extruder in S3 is 270°C.
[0044] In order to improve the uniformity of dispersion of glass fiber in nylon and solve the problem of broken strands, the inventors found during the experiment that when the head temperature of the screw extruder is 260-270°C, especially when the head temperature is 270°C and the temperature in the barrel of the screw extruder is 275°C, the uniformity of dispersion of glass fiber in nylon can be improved. The possible reason is that the friction heat of high-content glass fiber in the barrel of the screw extruder is used to cool down the head, which has the effect of building pressure in the barrel, so that the glass fiber can be better dispersed in the fluid nylon and achieve a uniform dispersion effect, further solving the problem of broken strands.
[0045] Beneficial Effects
[0046] 1. The high-rigidity nylon composite material provided by the present invention can improve the application of its products around automobile parts, reduce the weight of parts, achieve lightweight automobile parts, and reduce automobile energy consumption.
[0047] 2. The present invention uses aliphatic nylon and aromatic nylon in combination with high-content glass fiber to better embed the glass fiber into the gaps between molecular chain segments, forming a strong cross structure, thereby improving the strength performance of the nylon composite material.
[0048] 3. The high-rigidity nylon composite material provided by the present invention can disperse glass fibers into nylon in a fluid state, thereby achieving a better dispersion effect and reducing the strong shearing effect of the screw in the screw extruder on the glass fibers.
[0049] 4. The present invention solves the problem of broken strands by better dispersing high-content glass fibers into nylon, thereby obtaining a high-rigidity nylon composite material.
[0050] 5. The high-rigidity nylon composite material provided by the present invention can make the glass fiber dispersed better in the fluid nylon and achieve a uniform dispersion effect, thus solving the problem of broken fibers. DETAILED DESCRIPTION
[0051] Example 1
[0052] The first aspect of the present embodiment provides a high-rigidity nylon composite material, and its preparation raw materials include, by weight: 40 parts of aliphatic nylon, 5 parts of aromatic nylon, 50 parts of glass fiber, 3 parts of lubricant, 3 parts of dispersant, 0.3 parts of light stabilizer, and 0.6 parts of antioxidant.
[0053] The aliphatic nylon is nylon 66.
[0054] The aromatic nylon is nylon 6I / 6T.
[0055] The nylon 66 that can be purchased is model 2400, and the manufacturer is Shenma Industrial Co., Ltd.
[0056] The manufacturer model of the nylon 6I / 6T that can be purchased is DuPont 3426.
[0057] The grade of the glass fiber is ECS 301HP, and the manufacturer purchased is Chongqing International Composite Materials Co., Ltd.
[0058] The model of the lubricant is CYD-816A, and the manufacturer purchased is Weihai Chenyuan Molecular New Materials Co., Ltd.
[0059] The model of the dispersant is HyPer C182, and the manufacturer purchased is Wuhan Hyperbranched Resin Technology Co., Ltd.
[0060] The model of the light stabilizer is Tinuvin 234, and the manufacturer purchased is BASF.
[0061] The antioxidants include models 1096 and 168, and the weight ratio of antioxidant 1096 to antioxidant 168 is 1:1.
[0062] The antioxidant 1096 and antioxidant 168 were purchased from manufacturers including BASF.
[0063] A second aspect of the present embodiment provides a method for preparing a high-rigidity nylon composite material, comprising the following steps:
[0064] S1. Mixing aliphatic nylon with additives to obtain material a;
[0065] S2. The aromatic nylon is mixed with material a to obtain material b;
[0066] S3. Add material b and glass fiber into a screw extruder respectively for blending and extrusion to obtain a high-rigidity nylon composite material.
[0067] In S3, material b is added into the screw extruder through the main feeding port of the screw extruder, and the glass fiber is added into the screw extruder through the side feeding port of the screw extruder. After blending, extrusion, belt drawing, cooling, drying and pelletizing, a high-rigidity nylon composite material is obtained.
[0068] The side feed port uses a ZME threaded element.
[0069] During the blending and extrusion in S3, the temperature inside the barrel of the screw extruder is 275°C.
[0070] When performing the blending extrusion in S3, the vacuum degree in the barrel of the screw extruder is set to -0.065 MPa.
[0071] The hole diameter of the die orifice plate of the screw extruder in S3 is 2.5 mm.
[0072] The head temperature of the screw extruder in S3 is 270°C.
[0073] The screw extruder is a twin-screw extruder.
[0074] Example 2
[0075] The first aspect of the present embodiment provides a high-rigidity nylon composite material, and its preparation raw materials include, by weight: 40 parts of aliphatic nylon, 10 parts of aromatic nylon, 50 parts of glass fiber, 3 parts of lubricant, 3 parts of dispersant, 0.3 parts of light stabilizer, and 0.6 parts of antioxidant.
[0076] The aliphatic nylon is nylon 66.
[0077] The aromatic nylon is nylon 6I / 6T.
[0078] The model of nylon 66 purchased is 2400, and the manufacturer is Shenma Industrial Co., Ltd.
[0079] The manufacturer model of the nylon 6I / 6T that can be purchased is DuPont 3426.
[0080] The glass fiber is purchased with a brand name of ECS 301HP and is purchased from Chongqing International Composite Materials Co., Ltd.
[0081] The model of the lubricant is CYD-816A, and the manufacturer purchased is Weihai Chenyuan Molecular New Materials Co., Ltd.
[0082] The model of the dispersant is HyPer C182, and the manufacturer purchased is Wuhan Hyperbranched Resin Technology Co., Ltd.
[0083] The model of the light stabilizer is Tinuvin 234, and the manufacturer purchased is BASF.
[0084] The antioxidants include models 1096 and 168, and the weight ratio of antioxidant 1096 to antioxidant 168 is 1:1.
[0085] The antioxidant 1096 and antioxidant 168 were purchased from manufacturers including BASF.
[0086] A second aspect of the present embodiment provides a method for preparing a high-rigidity nylon composite material, comprising the following steps:
[0087] S1. Mixing aliphatic nylon with additives to obtain material a;
[0088] S2. The aromatic nylon is mixed with material a to obtain material b;
[0089] S3. Add material b and glass fiber into a screw extruder respectively for blending and extrusion to obtain a high-rigidity nylon composite material.
[0090] In S3, material b is added into the screw extruder through the main feeding port of the screw extruder, and the glass fiber is added into the screw extruder through the side feeding port of the screw extruder. After blending, extrusion, belt drawing, cooling, drying and pelletizing, a high-rigidity nylon composite material is obtained.
[0091] The side feed port uses a ZME threaded element.
[0092] During the blending and extrusion in S3, the temperature inside the barrel of the screw extruder is 275°C.
[0093] When performing the blending extrusion in S3, the vacuum degree in the barrel of the screw extruder is set to -0.065 MPa.
[0094] The hole diameter of the die orifice plate of the screw extruder in S3 is 2.5 mm.
[0095] The head temperature of the screw extruder in S3 is 270°C.
[0096] The screw extruder is a twin-screw extruder.
[0097] Example 3
[0098] The first aspect of the present embodiment provides a high-rigidity nylon composite material, and its preparation raw materials include, by weight: 40 parts of aliphatic nylon, 15 parts of aromatic nylon, 50 parts of glass fiber, 3 parts of lubricant, 3 parts of dispersant, 0.3 parts of light stabilizer, and 0.6 parts of antioxidant.
[0099] The aliphatic nylon is nylon 66.
[0100] The aromatic nylon is nylon 6I / 6T.
[0101] The model of nylon 66 purchased is 2400, and the manufacturer is Shenma Industrial Co., Ltd.
[0102] The manufacturer model of the nylon 6I / 6T purchased is DuPont 3426.
[0103] The glass fiber is purchased with a brand name of ECS 301HP and is purchased from Chongqing International Composite Materials Co., Ltd.
[0104] The model of the lubricant is CYD-816A, and the manufacturer purchased is Weihai Chenyuan Molecular New Materials Co., Ltd.
[0105] The model of the dispersant is HyPer C182, and the manufacturer purchased is Wuhan Hyperbranched Resin Technology Co., Ltd.
[0106] The model of the light stabilizer is Tinuvin 234, and the manufacturer purchased is BASF.
[0107] The antioxidants include models 1096 and 168, and the weight ratio of antioxidant 1096 to antioxidant 168 is 1:1.
[0108] The antioxidant 1096 and antioxidant 168 were purchased from manufacturers including BASF.
[0109] A second aspect of the present embodiment provides a method for preparing a high-rigidity nylon composite material, comprising the following steps:
[0110] S1. Mixing aliphatic nylon with additives to obtain material a;
[0111] S2. The aromatic nylon is mixed with material a to obtain material b;
[0112] S3. Add material b and glass fiber into a screw extruder respectively for blending and extrusion to obtain a high-rigidity nylon composite material.
[0113] In S3, material b is added into the screw extruder through the main feeding port of the screw extruder, and the glass fiber is added into the screw extruder through the side feeding port of the screw extruder. After blending, extrusion, belt drawing, cooling, drying and pelletizing, a high-rigidity nylon composite material is obtained.
[0114] The side feed port uses a ZME threaded element.
[0115] During the blending and extrusion in S3, the temperature inside the barrel of the screw extruder is 275°C.
[0116] When performing the blending extrusion in S3, the vacuum degree in the barrel of the screw extruder is set to -0.065 MPa.
[0117] The hole diameter of the die orifice plate of the screw extruder in S3 is 2.5 mm.
[0118] The head temperature of the screw extruder in S3 is 270°C.
[0119] The screw extruder is a twin-screw extruder.
[0120] Example 4
[0121] A first aspect of the present embodiment provides a high-rigidity nylon composite material, wherein the raw materials for its preparation include, by weight: 40 parts of aliphatic nylon, 50 parts of glass fiber, 3 parts of lubricant, 3 parts of dispersant, 0.3 parts of light stabilizer, and 0.6 parts of antioxidant.
[0122] The aliphatic nylon is nylon 66.
[0123] The model of nylon 66 purchased is 2400, and the manufacturer is Shenma Industrial Co., Ltd.
[0124] The glass fiber is purchased with a brand name of ECS 301HP and is purchased from Chongqing International Composite Materials Co., Ltd.
[0125] The model of the lubricant is CYD-816A, and the manufacturer purchased is Weihai Chenyuan Molecular New Materials Co., Ltd.
[0126] The model of the dispersant is HyPer C182, and the manufacturer purchased is Wuhan Hyperbranched Resin Technology Co., Ltd.
[0127] The model of the light stabilizer is Tinuvin 234, and the manufacturer purchased is BASF.
[0128] The antioxidants include models 1096 and 168, and the weight ratio of antioxidant 1096 to antioxidant 168 is 1:1.
[0129] The antioxidant 1096 and antioxidant 168 were purchased from manufacturers including BASF.
[0130] A second aspect of the present embodiment provides a method for preparing a high-rigidity nylon composite material, comprising the following steps:
[0131] S1. Mixing aliphatic nylon with additives to obtain material a;
[0132] S2. Add material a and glass fiber into a screw extruder respectively for blending and extrusion to obtain a high-rigidity nylon composite material.
[0133] In S2, material a is added into the screw extruder through the main feeding port of the screw extruder, and the glass fiber is added into the screw extruder through the side feeding port of the screw extruder. After blending, extrusion, belt drawing, cooling, drying and pelletizing, a high-rigidity nylon composite material is obtained.
[0134] The side feed port uses a ZME threaded element.
[0135] During the blending and extrusion in S2, the temperature inside the barrel of the screw extruder is 275°C.
[0136] When performing the blending extrusion in S2, the vacuum degree in the barrel of the screw extruder is set to -0.065 MPa.
[0137] The hole diameter of the die orifice plate of the screw extruder in S2 is 2.5 mm.
[0138] The head temperature of the screw extruder in S2 is 270°C.
[0139] The screw extruder is a twin-screw extruder.
[0140] Example 5
[0141] A first aspect of the present embodiment provides a high-rigidity nylon composite material, wherein the raw materials for its preparation include, by weight: 40 parts of aromatic nylon, 50 parts of glass fiber, 3 parts of lubricant, 3 parts of dispersant, 0.3 parts of light stabilizer, and 0.6 parts of antioxidant.
[0142] The aromatic nylon is nylon 6I / 6T.
[0143] The manufacturer model of the nylon 6I / 6T that can be purchased is DuPont 3426.
[0144] The glass fiber can be purchased under the brand name ECS 301HP, and the manufacturer is Chongqing International Composite Materials Co., Ltd.
[0145] The model of the lubricant is CYD-816A, and the manufacturer purchased is Weihai Chenyuan Molecular New Materials Co., Ltd.
[0146] The model of the dispersant is HyPer C182, and the manufacturer purchased is Wuhan Hyperbranched Resin Technology Co., Ltd.
[0147] The model of the light stabilizer is Tinuvin 234, and the manufacturer purchased is BASF.
[0148] The antioxidants include models 1096 and 168, and the weight ratio of antioxidant 1096 to antioxidant 168 is 1:1.
[0149] The antioxidant 1096 and antioxidant 168 were purchased from manufacturers including BASF.
[0150] A second aspect of the present embodiment provides a method for preparing a high-rigidity nylon composite material, comprising the following steps:
[0151] S1. The aromatic nylon and the additive are mixed to obtain material b;
[0152] S2. Add material b and glass fiber into a screw extruder respectively for blending and extrusion to obtain a high-rigidity nylon composite material.
[0153] In S2, material b is added into the screw extruder through the main feeding port of the screw extruder, and the glass fiber is added into the screw extruder through the side feeding port of the screw extruder. After blending, extrusion, belt drawing, cooling, drying and pelletizing, a high-rigidity nylon composite material is obtained.
[0154] The side feed port uses a ZME threaded element.
[0155] During the blending and extrusion in S2, the temperature inside the barrel of the screw extruder is 275°C.
[0156] When performing the blending extrusion in S2, the vacuum degree in the barrel of the screw extruder is set to -0.065 MPa.
[0157] The hole diameter of the die orifice plate of the screw extruder in S2 is 2.5 mm.
[0158] The head temperature of the screw extruder in S2 is 270°C.
[0159] The screw extruder is a twin-screw extruder.
[0160] Example 6
[0161] A first aspect of the present embodiment provides a high-rigidity nylon composite material, wherein the raw materials for its preparation include, by weight: 40 parts of nylon 66, 10 parts of nylon 6, 50 parts of glass fiber, 3 parts of lubricant, 3 parts of dispersant, 0.3 parts of light stabilizer, and 0.6 parts of antioxidant.
[0162] The model of nylon 66 purchased is 2400, and the manufacturer is Shenma Industrial Co., Ltd.
[0163] The model of the nylon 6 purchased is J2700, and the manufacturer is Hangzhou Juheshun New Materials Co., Ltd.
[0164] The glass fiber is purchased with a brand name of ECS 301HP and is purchased from Chongqing International Composite Materials Co., Ltd.
[0165] The model of the lubricant is CYD-816A, and the manufacturer purchased is Weihai Chenyuan Molecular New Materials Co., Ltd.
[0166] The model of the dispersant is HyPer C182, and the manufacturer purchased is Wuhan Hyperbranched Resin Technology Co., Ltd.
[0167] The model of the light stabilizer is Tinuvin 234, and the manufacturer purchased is BASF.
[0168] The antioxidants include models 1096 and 168, and the weight ratio of antioxidant 1096 to antioxidant 168 is 1:1.
[0169] The antioxidant 1096 and antioxidant 168 were purchased from manufacturers including BASF.
[0170] A second aspect of the present embodiment provides a method for preparing a high-rigidity nylon composite material, comprising the following steps:
[0171] S1. Mixing nylon 66 with an additive to obtain material a;
[0172] S2. Mixing nylon 6 with material a to obtain material b;
[0173] S3. Add material b and glass fiber into a screw extruder respectively for blending and extrusion to obtain a high-rigidity nylon composite material.
[0174] In S3, material b is added into the screw extruder through the main feeding port of the screw extruder, and the glass fiber is added into the screw extruder through the side feeding port of the screw extruder. After blending, extrusion, belt drawing, cooling, drying and pelletizing, a high-rigidity nylon composite material is obtained.
[0175] The side feed port uses a ZME threaded element.
[0176] During the blending and extrusion in S3, the temperature inside the barrel of the screw extruder is 275°C.
[0177] When performing the blending extrusion in S3, the vacuum degree in the barrel of the screw extruder is set to -0.065 MPa.
[0178] The hole diameter of the die orifice plate of the screw extruder in S3 is 2.5 mm.
[0179] The head temperature of the screw extruder in S3 is 270°C.
[0180] The screw extruder is a twin-screw extruder.
[0181] Example 7
[0182] The first aspect of the present embodiment provides a high-rigidity nylon composite material, and its preparation raw materials include, by weight: 40 parts of aliphatic nylon, 10 parts of aromatic nylon, 50 parts of glass fiber, 3 parts of lubricant, 3 parts of dispersant, 0.3 parts of light stabilizer, and 0.6 parts of antioxidant.
[0183] The aliphatic nylon is nylon 66.
[0184] The aromatic nylon is nylon 6I / 6T.
[0185] The model of nylon 66 purchased is 2400, and the manufacturer is Shenma Industrial Co., Ltd.
[0186] The manufacturer model of the nylon 6I / 6T purchased is DuPont 3426.
[0187] The glass fiber is purchased with a brand name of ECS 301HP and is purchased from Chongqing International Composite Materials Co., Ltd.
[0188] The model of the lubricant is CYD-816A, and the manufacturer purchased is Weihai Chenyuan Molecular New Materials Co., Ltd.
[0189] The model of the dispersant is HyPer C182, and the manufacturer purchased is Wuhan Hyperbranched Resin Technology Co., Ltd.
[0190] The model of the light stabilizer is Tinuvin 234, and the manufacturer purchased is BASF.
[0191] The antioxidants include models 1096 and 168, and the weight ratio of antioxidant 1096 to antioxidant 168 is 1:1.
[0192] The antioxidant 1096 and antioxidant 168 can be purchased from manufacturers including BASF.
[0193] A second aspect of the present embodiment provides a method for preparing a high-rigidity nylon composite material, comprising the following steps:
[0194] S1. Mixing aliphatic nylon with additives to obtain material a;
[0195] S2. The aromatic nylon is mixed with material a to obtain material b;
[0196] S3. Add material b and glass fiber into a screw extruder respectively for blending and extrusion to obtain a high-rigidity nylon composite material.
[0197] In S3, material b is added into the screw extruder through the main feeding port of the screw extruder, and the glass fiber is added into the screw extruder through the side feeding port of the screw extruder. After blending, extrusion, belt drawing, cooling, drying and pelletizing, a high-rigidity nylon composite material is obtained.
[0198] During the blending and extrusion in S3, the temperature inside the barrel of the screw extruder is 275°C.
[0199] When performing the blending extrusion in S3, the vacuum degree in the barrel of the screw extruder is set to -0.065 MPa.
[0200] The hole diameter of the die orifice plate of the screw extruder in S3 is 3 mm.
[0201] The head temperature of the screw extruder in S3 is 275°C.
[0202] The screw extruder is a twin-screw extruder.
[0203] Performance Testing
[0204] 1. Extrusion effect
[0205] It was observed whether the problem of strip breakage would occur during the extrusion and drawing process of preparing the high-rigidity nylon composite material in Examples 1-7. The test results are shown in Table 1.
[0206] 2. Tensile strength test
[0207] The tensile strength of the high rigidity nylon composite materials provided in Examples 1-7 was tested according to ISO 527-1-2012. The number of test samples provided in each example was greater than or equal to 5. The maximum and minimum values of the test results were removed and the average value was taken. The test results are shown in Table 1.
[0208] 3. Bending strength test
[0209] The high rigidity nylon composite materials provided in Examples 1-7 were tested for flexural strength in accordance with ISO 178-2019. The number of test samples provided in each example was greater than or equal to 5. The maximum and minimum values of the test results were removed and the average value was taken. The test results are shown in Table 1.
[0210] 4. Flexural modulus test
[0211] The high rigidity nylon composite materials provided in Examples 1-7 were tested for their flexural modulus in accordance with ISO 178-2019. The number of test samples provided in each example was greater than or equal to 5. The maximum and minimum values of the test results were removed and the average value was taken. The test results are shown in Table 1.
[0212] 5. Notched impact strength test
[0213] The notched impact strength of the high rigidity nylon composite materials provided in Examples 1-7 was tested according to ISO 179-1-2023. The number of test samples provided in each example was greater than or equal to 5. The maximum and minimum values of the test results were removed and the average value was taken. The test results are shown in Table 1.
[0214] Table 1
[0215]
[0216]
Claims
1. A high-rigidity nylon composite material, characterized in that: The raw materials for its preparation include, by weight: 40-60 parts of nylon, 40-50 parts of glass fiber, and 4.3-9.5 parts of auxiliary agent, wherein the nylon includes aliphatic nylon and aromatic nylon.
2. The high-rigidity nylon composite material according to claim 1, characterized in that: The aliphatic nylon is selected from one or more combinations of nylon 66, nylon 6, and nylon 610.
3. The high-rigidity nylon composite material according to claim 1, characterized in that: The aromatic nylon is selected from one or more combinations of nylon 6I / 6T, nylon 6T, nylon 9T and nylon 10T.
4. The high-rigidity nylon composite material according to any one of claims 1 to 3, characterized in that: The diameter of the glass fiber is 1 to 50 μm, and the length of the glass fiber is 1 to 5 mm.
5. The high-rigidity nylon composite material according to claim 1, characterized in that: The auxiliary agent is selected from a combination of one or more of a lubricant, a dispersant, a light stabilizer and an antioxidant.
6. A method for preparing a high-rigidity nylon composite material as claimed in claim 1, characterized in that: The following steps are involved: S1. Mixing aliphatic nylon with additives to obtain material a; S2. The aromatic nylon is mixed with material a to obtain material b; S3. Add material b and glass fiber into a screw extruder respectively for blending and extrusion to obtain a high-rigidity nylon composite material.
7. The method for preparing a high-rigidity nylon composite material according to claim 6, characterized in that: During the blending and extrusion in S3, the temperature inside the barrel of the screw extruder is 250-300°C.
8. The method for preparing a high-rigidity nylon composite material according to claim 6, characterized in that: When performing the blending extrusion in S3, the vacuum degree in the barrel of the screw extruder is set to -0.01 to -0.4 MPa.
9. The method for preparing a high-rigidity nylon composite material according to claim 6, characterized in that: The hole diameter of the die orifice plate of the screw extruder in S3 is 2 to 2.9 mm.
10. The method for preparing a high-rigidity nylon composite material according to claim 6, characterized in that: The head temperature of the screw extruder in S3 is 260-270°C.