Aluminum alloy door and window decorative material and manufacturing process thereof
通过使用硅酮密封胶,结合木纤维和玻璃纤维的添加,解决了铝合金门窗密封条老化和腐蚀问题,提高了密封性能和耐候性,延长了使用寿命,并降低了生产成本,适用于建筑 and home improvement field.
Patent Information
- Application Number
- CN202410953686.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-11-12
AI Technical Summary
Existing aluminum alloy door and window sealing strips are prone to aging, shrinking or falling off, resulting in a degradation of sealing performance. Long-term exposure to harsh environments may lead to surface corrosion, affecting aesthetics and service life.
Silicone sealant is made of raw materials such as polydimethylsiloxane, glass fiber, wood fiber, quartz powder, tapioca oil, glycerin, aminopropyltriethoxysilane and aluminum chloride, and is stabilized through vacuum reaction and The process generates, increasing wood fiber and glass fiber for improved bonding and weather resistance, and cassava oil and glycerin improve flexibility and bonding.
It significantly improves the adhesion, weather resistance and durability of sealant, extends service life, reduces production costs, is environmentally friendly and sustainable, and is suitable for architectural curtain walls and doors and windows.
Smart Images

Figure CN118931184A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of construction and home decoration, and in particular to an aluminum alloy door and window decoration material and a manufacturing process thereof. Background Art
[0002] Aluminum alloy door and window decoration materials mainly include ordinary aluminum alloy doors and windows, broken bridge aluminum alloy doors and windows, system doors and windows, aluminum clad wood doors and windows, etc. These materials have been widely used in the fields of construction and home decoration due to their light weight, firmness and non-deformation characteristics.
[0003] Ordinary aluminum alloy doors and windows are made of aluminum alloy extruded profiles, and their surfaces are treated by spraying or electrophoresis to adapt to different building shapes and interior decoration styles. Broken bridge aluminum alloy doors and windows use broken bridge technology, which improves the thermal insulation performance of doors and windows by adding insulation strips to aluminum alloy profiles. System doors and windows refer to a door and window system composed of a complete set of systematic doors and windows, including profiles, hardware accessories, sealing materials, etc., with the characteristics of high performance and high reliability. Aluminum clad wood doors and windows are made of wood and aluminum alloy, which not only maintains the advantages of aluminum alloy, but also adds better thermal insulation and sound insulation performance.
[0004] The manufacturing process of aluminum alloy doors and windows includes multiple steps. The first is frame and sash cutting, which is to cut the aluminum alloy profile into the required length. Next is milling, which is to process the profile through milling equipment to install hardware and glass. Then there is hardware installation, which is to install the hardware accessories required for doors and windows on the profile. Next is glass installation, which is to fix the glass to the window frame. Finally, there is sealant strip assembly, which is installed between the window frame and the window sash to improve the sealing performance. Throughout the manufacturing process, precision control is very critical to ensure that the size and structure of the product meet the design requirements.
[0005] However, in actual use, the sealing strip will age, shrink or fall off, resulting in a decrease in sealing performance. In addition, inaccurate installation may also cause gaps, which in turn affects the overall sealing effect. In addition, although aluminum alloy materials are corrosion-resistant, long-term exposure to harsh environments such as acid rain or seawater erosion may still cause surface corrosion or oxidation, affecting the appearance and service life of doors and windows. Summary of the invention
[0006] 1. Technical issues to be resolved
[0007] In view of the deficiencies in the prior art, the present invention provides an aluminum alloy door and window decoration material and a manufacturing process thereof, which has the advantages of strong sealing and long service life, and solves the problems of poor sealing and short service life.
[0008] (II) Technical solution
[0009] To achieve the above purpose, the present invention provides the following technical solution: its raw materials are composed of polydimethylsiloxane, filler, plasticizer, coupling agent and catalyst, and the weight ratio of the raw materials is: 50-60 parts of polydimethylsiloxane; 3-5 parts of glass fiber; 2-4 parts of wood fiber; 2-4 parts of quartz powder; 3-5 parts of cassava oil; 4-6 parts of glycerol; 3-5 parts of aminopropyltriethoxysilane; 3-5 parts of epoxysilane; 0.3-0.6 parts of aluminum chloride.
[0010] Preferably, the filler is glass fiber, wood fiber and quartz powder, the plasticizer is cassava oil and glycerol, the coupling agent is aminopropyltriethoxysilane and epoxysilane, and the catalyst is aluminum chloride.
[0011] Preferably, the method comprises the following steps:
[0012] Step 1. Raw material preparation: polydimethylsiloxane, glass fiber, wood fiber, quartz powder, cassava oil, glycerin, aminopropyl triethoxysilane, epoxy silane and aluminum chloride are selected as raw materials;
[0013] Step 2: Mix evenly: Mix the raw materials according to the proportion;
[0014] Step 3, reaction control: put the mixed raw materials into a vacuum reactor, set the reactor temperature to 200°C, and keep the agitator in a vacuum stirring state until the reaction is completed;
[0015] Step 4, post-treatment: After the reaction is completed, cooling and stabilization treatment are performed at room temperature with a humidity of 90% to generate a silicone sealant;
[0016] Step 5: Quality inspection: Conduct quality inspection on the produced silicone sealant;
[0017] Step 6: Packaging and storage: The silicone sealant that passes the inspection is packaged and stored.
[0018] Preferably, the production process of the wood fiber is:
[0019] S1.1, Raw material preparation: select 10-year-old camphor wood as raw material, and then crush, dry and screen it;
[0020] S1.2, Fiber extraction: Separation of cellulose fibers using thermodynamic methods;
[0021] S1.3, fiber processing: the extracted fiber was placed in an oven and dried at a constant temperature of 90°C for 4 hours.
[0022] Preferably, in the raw material preparation stage, S1.1 uses a grinder to grind the cut camphor wood segments, and then puts the crushed wood chips into an oven and drys them at 120° C. for 2 hours.
[0023] Preferably, the operation process of the S1.2 thermodynamic method is:
[0024] S2.1, steaming: soak the dried sawdust in water vapor at a temperature of 300°C and a pressure of 150 for 1.5 to 3 hours;
[0025] S2.2, Pyrolysis: Dry the soaked sawdust, put it into a thermogravimetric analyzer, and increase the instrument temperature from room temperature to 1273K. After 1 hour, take it out and cool it down.
[0026] Preferably, the stabilization treatment in step 4 refers to the process in which the raw materials of the mixture after the reaction is complete react with moisture in the air to achieve solidification and form a silicone sealant.
[0027] Preferably, the production process of the cassava oil is:
[0028] S3.1. Peeling and slicing: The cassava needs to be peeled and cut into slices;
[0029] S3.2, cooking and ripening: the peeled cassava slices are boiled in distilled water at 100°C for 2 hours;
[0030] S3.3, sun-drying and pounding: the cooked cassava chips are sun-dried, and a blender is used to pound the dried cassava chips into cassava flour;
[0031] S3.4. Extracting oil: Send the cassava flour into an extruder for squeezing, and separate the oil component therein to obtain cassava oil.
[0032] Preferably, the raw materials are composed of 55 parts by weight of polydimethylsiloxane, 3 parts of glass fiber, 2 parts of wood fiber, 4 parts of quartz powder, 4 parts of cassava oil, 5 parts of glycerol, 3 parts of aminopropyltriethoxysilane, 4 parts of epoxysilane and 0.4 parts of aluminum chloride.
[0033] Preferably, the raw materials are composed of 54 parts by weight of polydimethylsiloxane, 5 parts by weight of glass fiber, 4 parts by weight of wood fiber, 2 parts by weight of quartz powder, 5 parts by weight of cassava oil, 6 parts by weight of glycerol, 4 parts by weight of aminopropyltriethoxysilane, 3 parts by weight of epoxysilane, and 0.6 parts by weight of aluminum chloride.
[0034] Compared with the prior art, the present invention provides an aluminum alloy door and window decoration material and a manufacturing process thereof, which has the following beneficial effects:
[0035] 1. The present invention adds wood fiber and glass fiber to silicone sealant to enhance the adhesive force and weather resistance of the sealant. Wood fiber and glass fiber can increase the contact area between the sealant and various materials, thereby improving its adhesive strength, which is particularly important for places that need to withstand a certain force or prevent moisture penetration; the addition of glass fiber and wood fiber can improve the weather resistance of the sealant, making it more stable when exposed to changes in the external environment, and not prone to cracking or falling off due to factors such as temperature differences and humidity; these two fibers themselves have good flexibility. When the sealant is subjected to external forces, the fibers can absorb part of the stress and reduce the generation of cracks , improve the overall crack resistance of the sealant; the addition of wood fiber and glass fiber helps to increase the service life of the sealant, enabling it to maintain the sealing effect for a longer period of time and reduce the frequency of maintenance and replacement; by adding these two fibers, the production cost of silicone sealant can be reduced without sacrificing performance, thereby improving the cost performance of the product; using natural wood fiber and glass fiber as additives is more environmentally friendly and sustainable than other synthetic materials. Combining the above operations, adding wood fiber and glass fiber to silicone sealant can improve its comprehensive performance, including adhesion, weather resistance and durability, while also helping to reduce costs and improve environmental protection.
[0036] 2. The present invention adds cassava oil and glycerin to the silicone sealant. The cassava oil and glycerin can act as softeners to increase the flexibility of the silicone sealant, making it less likely to crack under temperature changes or external forces and maintaining good sealing performance; the silicone sealant itself has excellent weather resistance, and the addition of cassava oil and glycerin can further improve its weather resistance and extend its service life; glycerin has a certain viscosity, which can enhance the adhesion between the silicone sealant and various substrates and improve its bonding effect on different materials; the addition of cassava oil and glycerin can improve the processing performance of the silicone sealant, making it easier to operate during the construction process and reducing problems such as bubbles and glue breakage. Occurrence; As a natural vegetable oil, the use of cassava oil helps to reduce the impact on the environment, which is in line with the current development trend of green building materials; Compared with other additives, cassava oil and glycerin are low in cost, which helps to reduce the overall production cost of silicone sealants without sacrificing performance. Combining the above advantages, adding cassava oil and glycerin to silicone sealants can bring many benefits, including improved flexibility, enhanced weather resistance, enhanced adhesion, optimized processing performance, environmental sustainability and reduced costs. These improvements help to improve the overall performance of silicone sealants and make their application in building curtain walls, insulating glass, doors and windows more extensive and effective. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 It is a schematic diagram of the structure of the present invention; DETAILED DESCRIPTION
[0038] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0039] See also Figure 1 The raw materials are composed of polydimethylsiloxane, filler, plasticizer, coupling agent and catalyst, and the weight ratio of the raw materials is: 50-60 parts of polydimethylsiloxane; 3-5 parts of glass fiber; 2-4 parts of wood fiber; 2-4 parts of quartz powder; 3-5 parts of cassava oil; 4-6 parts of glycerol; 3-5 parts of aminopropyltriethoxysilane; 3-5 parts of epoxysilane; 0.3-0.6 parts of aluminum chloride.
[0040] Specifically, the filler is glass fiber, wood fiber and quartz powder, the plasticizer is cassava oil and glycerol, the coupling agent is aminopropyltriethoxysilane and epoxysilane, and the catalyst is aluminum chloride.
[0041] Specifically, the following steps are included:
[0042] Step 1. Raw material preparation: polydimethylsiloxane, glass fiber, wood fiber, quartz powder, cassava oil, glycerin, aminopropyl triethoxysilane, epoxy silane and aluminum chloride are selected as raw materials;
[0043] Step 2: Mix evenly: Mix the raw materials according to the proportion;
[0044] Step 3, reaction control: put the mixed raw materials into a vacuum reactor, set the reactor temperature to 200°C, and keep the agitator in a vacuum stirring state until the reaction is completed;
[0045] Step 4, post-treatment: After the reaction is completed, cooling and stabilization treatment are performed at room temperature with a humidity of 90% to generate a silicone sealant;
[0046] Step 5: Quality inspection: Conduct quality inspection on the produced silicone sealant;
[0047] Step 6: Packaging and storage: The silicone sealant that passes the inspection is packaged and stored.
[0048] Specifically, the production process of the wood fiber is as follows:
[0049] S1.1, Raw material preparation: Choose 10-year-old camphor wood as raw material, crush, dry and screen it, so that the subsequent production process can proceed smoothly;
[0050] S1.2, Fiber extraction: Separation of cellulose fibers using thermodynamic methods, which utilize steam to cook and extract wood to separate cellulose fibers;
[0051] S1.3, fiber processing: the extracted fiber was placed in an oven and dried at a constant temperature of 90°C for 4 hours.
[0052] Specifically, in the raw material preparation stage, S1.1 uses a grinder to grind the cut camphor wood segments, and then puts the crushed wood chips into an oven and drys them at 120° C. for 2 hours.
[0053] Specifically, the operation process of the S1.2 thermodynamic method is:
[0054] S2.1, steaming: soak the dried sawdust in water vapor at a temperature of 300°C and a pressure of 150 for 1.5 to 3 hours. In this step, the water vapor can penetrate into the cell wall and increase the degree of hydrolysis, thus facilitating the extraction of cellulose fibers;
[0055] S2.2, Pyrolysis: dry the soaked sawdust, put it into a thermogravimetric analyzer, and increase the instrument temperature from room temperature to 1273K. After 1 hour, take it out and cool it down. The temperature from room temperature to 1273K is divided into three stages: a small amount of hydroxyl release in the low-temperature stage, the main bond breakage and glycosidic bond opening breakage in the medium-temperature stage, and further decomposition in the high-temperature stage to produce smaller molecular fragments.
[0056] Specifically, the stabilization treatment in step 4 refers to the process in which the raw materials of the mixture after the reaction is complete react with moisture in the air to achieve solidification and form a silicone sealant.
[0057] Specifically, the production process of the cassava oil is:
[0058] S3.1. Peeling and slicing: The cassava needs to be peeled and cut into slices;
[0059] S3.2, cooking and ripening: the peeled cassava slices are boiled in distilled water at 100°C for 2 hours;
[0060] S3.3, sun-drying and pounding: the cooked cassava chips are sun-dried, and a blender is used to pound the dried cassava chips into cassava flour;
[0061] S3.4. Extracting oil: Send the cassava flour into an extruder for squeezing, and separate the oil component therein to obtain cassava oil.
[0062] Example 1
[0063] Specifically, the weight ratio of the raw materials is: 55 parts of polydimethylsiloxane; 3 parts of glass fiber; 2 parts of wood fiber; 4 parts of quartz powder; 4 parts of cassava oil; 5 parts of glycerol; 3 parts of aminopropyl triethoxysilane; 4 parts of epoxy silane; and 0.4 parts of aluminum chloride.
[0064] Example 2
[0065] Specifically, the weight ratio of the raw materials is: 54 parts of polydimethylsiloxane; 5 parts of glass fiber; 4 parts of wood fiber; 2 parts of quartz powder; 5 parts of cassava oil; 6 parts of glycerol; 4 parts of aminopropyl triethoxysilane; 3 parts of epoxy silane; and 0.6 parts of aluminum chloride.
[0066] The laboratory produced the finished product according to the raw material formula provided in Example 1-2, and applied it as a decorative material on aluminum alloy doors and windows through the following steps:
[0067] S4.1, Milling holes: Mill holes on the aluminum alloy profile for installing sealant;
[0068] S4.2. Install the sealing gasket and connector: Install the elastic gasket in the milled hole to ensure good contact and sealing effect between the sealant and the aluminum alloy profile, and then install the connector on the profile;
[0069] S4.3, profile mortise and tenon joint: connect the parts of the aluminum alloy profile by mortise and tenon joint to form a complete door and window frame structure, and tighten the profile after mortise and tenon joint to ensure the stability and sealing of the structure;
[0070] S4.4, mortise and tenon glue injection: inject the silicone sealant prepared in Example 1-2 into the mortise and tenon joint gap, which serves to enhance the waterproof, vibration-proof, leak-proof, sound-proof and heat-insulating properties of the structure;
[0071] S4.5, Peel test: Before using silicone sealant, conduct peel test with glass, profiles, and compatibility test with contacting organic materials;
[0072] S4.6, Curing process: After the sealant is injected, it takes a certain amount of time to cure, and the temperature is maintained at 40°C during the curing process;
[0073] S4.7, Inspection and finishing: After the sealant is cured, inspect the doors and windows to ensure that the sealant is evenly filled and has no defects, and make necessary finishing;
[0074] S4.8, Cleaning: After completing all processes, clean the doors and windows to remove excess sealant residue to ensure aesthetics.
[0075] The laboratory conducted several tests on the finished products used as decorative materials on aluminum alloy doors and windows in Examples 1-2, and recorded the test results in the following Table 1:
[0076] Test items Test conditions Test Results in conclusion Weather resistance Under ultraviolet light No significant changes qualified Bond Strength 22℃,54%RH 1.3MPa qualified Temperature resistance -25℃ to 90℃ No obvious cracks qualified Moisture resistance 96%RH No obvious mildew qualified Chemical resistance Immerse in 4% hydrochloric acid solution No obvious corrosion qualified
[0077] Note: The test duration is 24 hours.
[0078] Experimental conclusion:
[0079] Weather resistance: After being irradiated by ultraviolet light for 24 hours, there is no obvious change in the material, which shows that the decorative material has good weather resistance and can resist the long-term effects of ultraviolet light, and is suitable for outdoor environments;
[0080] Bond strength: Under standard environmental conditions (22°C temperature and 54% relative humidity), the bond strength of the material reaches 1.3MPa, exceeding the qualified standard, indicating that the material has sufficient bonding force to maintain the stability of the structure in actual use;
[0081] Temperature resistance: The material has no obvious cracks in the temperature range of -25℃ to 90℃, showing excellent temperature resistance and suitable for use in different climatic conditions;
[0082] Moisture resistance: After 24 hours in a high humidity environment of 96%, the material showed no obvious mildew, proving that it has good moisture resistance and is not easily damaged or moldy due to moisture;
[0083] Chemical resistance: After the material was immersed in 4% NaCl solution for 24 hours, there was no obvious corrosion phenomenon, indicating that it has a certain resistance to salt chemicals and is suitable for environments where it can be exposed to such substances;
[0084] In summary, the ketone sealant in Examples 1-2, when used as a decorative material on aluminum alloy doors and windows, passed all test items, exhibiting good weather resistance, bonding strength, temperature resistance, moisture resistance and chemical resistance, and met the requirements for being a decorative material for aluminum alloy doors and windows.
[0085] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. An aluminum alloy door and window decoration material and its manufacturing process, characterized in that: The raw materials are composed of polydimethylsiloxane, filler, plasticizer, coupling agent and catalyst, and the weight ratio of the raw materials is: 50-60 parts of polydimethylsiloxane; 3-5 parts of glass fiber; 2-4 parts of wood fiber; 2-4 parts of quartz powder; 3-5 parts of cassava oil; 4-6 parts of glycerin; 3-5 parts of aminopropyltriethoxysilane; 3-5 parts of epoxysilane; 0.3-0.6 parts of aluminum chloride.
2. The aluminum alloy door and window decoration material and its manufacturing process according to claim 1, characterized in that: The filler is glass fiber, wood fiber and quartz powder, the plasticizer is cassava oil and glycerol, the coupling agent is aminopropyl triethoxysilane and epoxy silane, and the catalyst is aluminum chloride.
3. A manufacturing process for aluminum alloy door and window decorative materials, characterized in that: The following steps are involved: Step 1. Raw material preparation: polydimethylsiloxane, glass fiber, wood fiber, quartz powder, cassava oil, glycerin, aminopropyl triethoxysilane, epoxy silane and aluminum chloride are selected as raw materials; Step 2: Mix evenly: Mix the raw materials according to the proportion; Step 3, reaction control: put the mixed raw materials into a vacuum reactor, set the reactor temperature to 200°C, and keep the agitator in a vacuum stirring state until the reaction is completed; Step 4, post-treatment: After the reaction is completed, cooling and stabilization treatment are performed at room temperature with a humidity of 90% to generate a silicone sealant; Step 5: Quality inspection: Conduct quality inspection on the produced silicone sealant; Step 6: Packaging and storage: The silicone sealant that passes the inspection is packaged and stored.
4. The aluminum alloy door and window decoration material and its manufacturing process according to claim 3, characterized in that: The production process of the wood fiber is as follows: S1.1, Raw material preparation: select 10-year-old camphor wood as raw material, and then crush, dry and screen it; S1.2, Fiber extraction: Separation of cellulose fibers using thermodynamic methods; S1.3, fiber processing: the extracted fiber was placed in an oven and dried at a constant temperature of 90°C for 4 hours.
5. The aluminum alloy door and window decoration material and its manufacturing process according to claim 4, characterized in that: In the step S1.1, during the raw material preparation stage, the cut camphor wood segments are crushed using a crusher, and the crushed wood chips are placed in an oven and dried at 120° C. for 2 hours.
6. The aluminum alloy door and window decoration material and the manufacturing process thereof according to claim 4, characterized in that: The operation process of the S1.2 thermodynamic method is: S2.1, steaming: soak the dried sawdust in water vapor at a temperature of 300°C and a pressure of 150 for 1.5 to 3 hours; S2.2, Pyrolysis: Dry the soaked sawdust, put it into a thermogravimetric analyzer, and increase the instrument temperature from room temperature to 1273K. After 1 hour, take it out and cool it down.
7. The aluminum alloy door and window decoration material and its manufacturing process according to claim 3, characterized in that: The stabilization treatment in step 4 refers to the process in which the raw materials of the mixture after the reaction is complete react with moisture in the air to achieve solidification and form a silicone sealant.
8. The aluminum alloy door and window decoration material and its manufacturing process according to claim 3, characterized in that: The preparation process of described cassava oil is: S3.
1. Peeling and slicing: The cassava needs to be peeled and cut into slices; S3.2, cooking and ripening: the peeled cassava slices are boiled in distilled water at 100°C for 2 hours; S3.3, sun-drying and pounding: the cooked cassava chips are sun-dried, and a blender is used to pound the dried cassava chips into cassava flour; S3.
4. Extracting oil: Send the cassava flour into an extruder for squeezing, and separate the oil component therein to obtain cassava oil.
9. The aluminum alloy door and window decoration material and its manufacturing process according to claim 1, characterized in that: The weight ratio of the raw materials is: 55 parts of polydimethylsiloxane; 3 parts of glass fiber; 2 parts of wood fiber; 4 parts of quartz powder; 4 parts of cassava oil; 5 parts of glycerol; 3 parts of aminopropyl triethoxy silane; 4 parts of epoxy silane; 0.4 parts of aluminum chloride.
10. The aluminum alloy door and window decoration material and the manufacturing process thereof according to claim 1, characterized in that: The weight ratio of the raw materials is: 54 parts of polydimethylsiloxane; 5 parts of glass fiber; 4 parts of wood fiber; 2 parts of quartz powder; 5 parts of cassava oil; 6 parts of glycerol; 4 parts of aminopropyl triethoxysilane; 3 parts of epoxy silane; 0.6 parts of aluminum chloride.