Titanium-oxygen-cluster-doped ultraviolet curing silicone oil as well as preparation method and application thereof

Through the mixing method of titanium oxide clusters and epoxy acrylic silica oil, the problems of uneven internal structure and low refractive index of ultraviolet cured silicone oil are solved, and the preparation of high refractive and high yields is achieved, which is suitable for functional elastic materials. , medical dressings and packaging materials.

CN118931193APending Publication Date: 2024-11-12JIANGXI RONGXIN TECH SILICON IND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411266452.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-10
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing ultraviolet cured silicone oil has problems such as uneven internal structure, low refractive index and high production costs.

Method used

The titanium oxide cluster and epoxy acrylic silica oil and solvent were used to achieve uniform modification of titanium oxide clusters and silicone materials through covalent bond linkage, and ultraviolet cured silicon oil doped with titanium oxide cluster was prepared.

Benefits of technology

The preparation of silicone oil with simple process, uniform internal structure and high refractive index is achieved, and the process yield is higher than 96%. The silicone oil is clear and transparent, and the color is consistent with the initial silicone oil.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118931193A_ABST
    Figure CN118931193A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of novel organic silicon materials, and discloses titanium-oxygen-cluster-doped ultraviolet curing silicone oil as well as a preparation method and application of the titanium-oxygen-cluster-doped ultraviolet curing silicone oil. The preparation method of the titanium-oxygen-cluster-doped ultraviolet curing silicone oil comprises the following step: mixing epoxy acrylic silicone oil, titanium-oxygen clusters and a solvent to prepare the titanium-oxygen-cluster-doped ultraviolet curing silicone oil. The prepared silicone oil is clear and transparent, and the color is consistent with that of initial silicone oil; the preparation method disclosed by the invention is simple and convenient in process, and the yield is greater than 96%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of new organosilicon materials, and in particular to a titanium oxide cluster-doped ultraviolet light-cured silicone oil and a preparation method and application thereof. Background Art

[0002] UV curing is a chemical process that uses ultraviolet light to irradiate the coating to produce radiation polymerization, radiation crosslinking and radiation grafting reactions, and quickly convert low molecular weight substances into high molecular weight products. Compared with several other commonly used photocuring methods, UV curing has the advantages of fast curing speed, solvent-free curing, low temperature curing and simple curing equipment. Photocurable silicone oil is widely used in functional elastomer materials, medical dressings and packaging materials due to its high transparency, good fluidity and easy coating. Acrylic silicone oil is an important component of photocurable silicone oil. Its curing principle is that the unsaturated double bonds produce free radical polymerization under the induction of free radical initiators that can absorb ultraviolet light, and then cure.

[0003] Adding metal oxides to silicone oil or silicone resin can improve the refractive index, thermal conductivity, heat resistance and other properties of the material. Commonly used metal oxides include nano zirconium dioxide (ZiO2), nano cerium dioxide (CeO2) and nano titanium dioxide (TiO2). There are two main methods for adding metal oxides to the material: 1) synthesizing nano metal oxides by sol-gel method, and then directly physically blending with silicone oil or silicone resin to obtain nano metal oxide modified silicone material; 2) mixing metal oxide basic raw materials with silane coupling agents, small molecule alkoxysilanes, etc. to obtain silicone modified nano metal oxides, and then physically mixing with silicone oil or silicone resin to obtain nano metal oxide modified silicone material. The preparation of the above materials by physical blending has the advantages of simple operation and easy scale-up production, but also has the disadvantages of uneven mixing causing uneven internal structure of the material, thereby affecting the overall performance of the material. How to achieve uniform combination of nano metal oxides and prepolymers is one of the difficulties in the current field.

[0004] In recent years, the research on titanium oxide clusters has developed rapidly. Titanium oxide clusters with rich core structures protected by various organic ligands have been reported one after another. They have been applied in catalysis, bioimaging and other fields, and their application scope is still expanding. Titanium oxide clusters have the following remarkable characteristics: (1) Most of them have good solubility; (2) They have atomically precise structures, with sizes between small molecules and nanoparticles, and their cores are the same or similar to the intrinsic structure of oxides; (3) The surface ligands are exchangeable, and the active functional groups on the ligands are easy to derivatize; these characteristics are very suitable for the modification of metal oxides and organosilicon materials. Through the easy exchangeability of ligands, they can be linked to organosilicon prepolymers in the form of covalent bonds, thereby achieving uniform modification of materials.

[0005] Therefore, it is of great significance to study a titanium oxide cluster-doped UV-curable silicone oil with simple process, uniform internal structure and high refractive index, as well as its preparation method and application. Summary of the invention

[0006] In view of this, the present invention provides a titanium oxide cluster doped UV-curable silicone oil and a preparation method and application thereof, the purpose of which is to solve the technical problems of uneven internal structure, low refractive index and high production cost of UV-curable silicone oil obtained by existing preparation methods.

[0007] In order to achieve the above object, the present invention adopts the following technical solution:

[0008] The present invention provides a method for preparing titanium oxide cluster-doped ultraviolet light-cured silicone oil, comprising the following steps:

[0009] Titanium oxide cluster-doped ultraviolet light-cured silicone oil is prepared by mixing epoxy acrylic silicone oil, titanium oxide clusters and solvent.

[0010] Preferably, the usage ratio of the epoxy acrylic silicone oil, the titanium oxide cluster and the solvent is 10g:0.5-3g:1-10mL.

[0011] Preferably, the epoxy acrylate silicone oil includes terminal epoxy acrylate silicone oil and / or side epoxy acrylate silicone oil.

[0012] Preferably, the titanium oxide cluster includes one or more of titanium oxide cluster Ti6, titanium oxide cluster Ti8, titanium oxide cluster Ti12 and titanium oxide cluster Ti32.

[0013] Preferably, the titanium oxide cluster Ti6 is Ti6O6(nPrCOO)6(OiPr)6, and the titanium oxide cluster Ti8 is Ti8O8(tBuCOO) 16 , titanium oxide cluster Ti12 is Ti 12 O 16 (OiPr) 16 , titanium oxide cluster Ti32 is Ti32, Ti 32 (m2-O)8(m3-O)8-(OCH2CH2O) 32 (RCOO) 16 (OCH2CH2OH) 16 , wherein R = one or any combination of ethyl, propenyl, and tert-butyl.

[0014] Preferably, the solvent is chloroform.

[0015] Preferably, the mixing time is 2 to 7 hours, and the mixing temperature is 20 to 80°C.

[0016] The invention also provides a method for preparing titanium oxide cluster-doped ultraviolet light-curing silicone oil, and titanium oxide cluster-doped ultraviolet light-curing silicone oil obtained by the method.

[0017] The present invention also provides the application of titanium oxide cluster doped ultraviolet light curing silicone oil in functional elastic materials, medical dressings and packaging materials.

[0018] It can be seen from the above technical solutions that, compared with the prior art, the present invention has the following beneficial effects:

[0019] The silicone oil prepared by the invention is clear and bright, and its color is consistent with that of the initial silicone oil; the preparation method of the invention has simple process and the yield is greater than 96%. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.

[0021] Figure 1 This is the structure diagram of the titanium oxide cluster Ti32, where the green balls are titanium atoms, the gray balls are carbon atoms, and the red balls are oxygen atoms;

[0022] Figure 2 It is a reaction schematic diagram of the present invention;

[0023] Figure 3 The hydrogen nuclear magnetic resonance spectra of the silicone oils obtained in Examples 1 to 4 are shown in FIG.

[0024] Figure 4 The infrared spectra of the silicone oils obtained in Examples 1 to 4 are shown in FIG. DETAILED DESCRIPTION

[0025] The present invention provides a method for preparing titanium oxide cluster-doped ultraviolet light-cured silicone oil, comprising the following steps:

[0026] Titanium oxide cluster-doped ultraviolet light-cured silicone oil is prepared by mixing epoxy acrylic silicone oil, titanium oxide clusters and solvent.

[0027] In the present invention, the usage ratio of the epoxy acrylic silicone oil, the titanium oxide cluster and the solvent is preferably 10g:0.5-3g:1-10mL, more preferably 10g:1-2.5g:3-8mL, and more preferably 10g:1.5-2g:5-6mL.

[0028] In the present invention, the epoxy acrylate silicone oil preferably includes terminal epoxy acrylate silicone oil and / or side epoxy acrylate silicone oil.

[0029] In the present invention, the titanium oxide cluster preferably includes one or more of titanium oxide cluster Ti6, titanium oxide cluster Ti8, titanium oxide cluster Ti12 and titanium oxide cluster Ti32.

[0030] In the present invention, the titanium oxide cluster Ti6 is preferably Ti6O6(nPrCOO)6(OiPr)6, and the titanium oxide cluster Ti8 is preferably Ti8O8(tBuCOO) 16 , the titanium oxide cluster Ti12 is preferably Ti 12 O 16 (OiPr) 16 , the titanium oxide cluster Ti32 is preferably Ti 32 (m2-O)8(m3-O)8-(OCH2CH2O) 32 (RCOO) 16 (OCH2CH2OH) 16 , wherein R = one or any combination of ethyl, propenyl, and tert-butyl.

[0031] In the present invention, the titanium oxide cluster is a prior art, and the specific materials can refer to the following documents: Xing C, Yingzi H, Jie F, et al. Ti-Oxo Clusters with Peripheral Alkyl Groups as Cathode Interlayers for Efficient Organic Solar Cells. [J]. ACS applied materials & interfaces, 2021, 13 (33) and Zhou Z, Chaowei Z, Yuefeng Z, et al. Surface tailored Ti-oxo clusters enabling highly efficient organic solar cells [J]. Chemical Engineering Journal, 2023, 454 (P2).

[0032] In the present invention, the solvent is preferably chloroform.

[0033] In the present invention, the mixing time is preferably 2 to 7 hours, more preferably 3 to 6 hours, more preferably 4 to 5 hours, and the mixing temperature is preferably 20 to 80°C, more preferably 30 to 70°C, more preferably 40 to 60°C.

[0034] In the present invention, the purpose of the mixing is to fully exchange the hydroxyl groups in the silicone oil with the surface ligands of the titanium oxide clusters.

[0035] In the present invention, after the mixing, reduced pressure distillation and vacuum drying are sequentially performed; the purpose of the reduced pressure distillation is to remove chloroform, and the purpose of the vacuum drying is to remove volatile components.

[0036] In the present invention, the vacuum drying time is preferably 100 to 140 min, more preferably 105 to 130 min, more preferably 110 to 120 min, and the vacuum drying temperature is preferably 55 to 65°C, more preferably 58 to 64°C, more preferably 60 to 62°C.

[0037] The invention also provides a method for preparing titanium oxide cluster-doped ultraviolet light-curing silicone oil, and titanium oxide cluster-doped ultraviolet light-curing silicone oil obtained by the method.

[0038] The present invention also provides the application of titanium oxide cluster doped ultraviolet light curing silicone oil in functional elastic materials, medical dressings and packaging materials.

[0039] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0040] In the embodiment of the present invention, the terminal epoxy acrylic silicone oil and the side epoxy acrylic silicone oil are both produced by Shandong Dayi Chemical Co., Ltd.

[0041] Example 1

[0042] Take 10 g of terminal epoxy acrylate silicone oil in a round-bottom flask, dissolve 0.5 g of titanium oxide cluster Ti32 (R group is tert-butyl) in 2 mL of chloroform, add it to the above round-bottom flask and mix it with the terminal epoxy acrylate silicone oil. After stirring at room temperature for 5 hours, remove the chloroform by vacuum distillation, and then vacuum dry it at 60°C for 120 minutes to remove the volatiles. The obtained silicone oil is clear and bright, and the color is consistent with the initial silicone oil. The weight is 10.4 g and the yield is 99.05%.

[0043] Example 2

[0044] Take 10 g of terminal epoxy acrylate silicone oil in a round-bottom flask, dissolve 1.0 g of titanium oxide cluster Ti32 (R group is tert-butyl) in 4 mL of chloroform, add it to the above round-bottom flask and mix it with the terminal epoxy acrylate silicone oil. After stirring at room temperature for 5 hours, remove the chloroform by vacuum distillation, and then vacuum dry it at 60°C for 120 minutes to remove the volatiles. The obtained silicone oil is clear and transparent, and the color is consistent with the initial silicone oil. The weight is 10.9 g and the yield is 99.09%.

[0045] Example 3

[0046] Take 10g of terminal epoxy acrylate silicone oil in a round-bottom flask, dissolve 1.5g of titanium oxide cluster Ti32 (R group is tert-butyl) in 5mL of chloroform, add it to the above round-bottom flask and mix it with the terminal epoxy acrylate silicone oil. After stirring at room temperature for 5h, remove the chloroform by vacuum distillation, and then vacuum dry it at 60℃ for 120min to remove the volatiles. The obtained silicone oil is clear and transparent, and the color is consistent with the initial silicone oil. The weight is 11.35g and the yield is 98.70%.

[0047] Example 4

[0048] Take 10 g of terminal epoxy acrylate silicone oil in a round-bottom flask, dissolve 2.0 g of titanium oxide cluster Ti32 (R group is tert-butyl) in 6 mL of chloroform, add it to the above round-bottom flask and mix it with the terminal epoxy acrylate silicone oil. After stirring at room temperature for 5 hours, remove the chloroform by vacuum distillation, and then vacuum dry it at 60°C for 120 minutes to remove the volatiles. The obtained silicone oil is clear and transparent, and the color is consistent with the initial silicone oil. The weight is 11.86 g and the yield is 98.83%.

[0049] Example 5

[0050] Take 10 g of terminal epoxy acrylate silicone oil in a round-bottom flask, dissolve 3.0 g of titanium oxide cluster Ti32 (R group is tert-butyl) in 10 mL of chloroform, add it to the above round-bottom flask and mix it with the terminal epoxy acrylate silicone oil. After stirring at room temperature for 5 hours, remove the chloroform by vacuum distillation, and then vacuum dry it at 60°C for 120 minutes to remove the volatiles. The obtained silicone oil is clear and transparent, and the color is consistent with the initial silicone oil. The weight is 12.60 g and the yield is 96.92%.

[0051] Example 6

[0052] Take 10 g of terminal epoxy acrylate silicone oil in a round-bottom flask, dissolve 1.0 g of titanium oxide cluster Ti6 in 3 mL of chloroform, add it to the above round-bottom flask and mix it with the terminal epoxy acrylate silicone oil. After stirring at room temperature for 5 hours, remove the chloroform by vacuum distillation, and then vacuum dry it at 60°C for 120 minutes to remove the volatiles. The obtained silicone oil is clear and bright, and the color is consistent with the initial silicone oil. The weight is 10.87 g and the yield is 98.92%.

[0053] Example 7

[0054] Take 10 g of terminal epoxy acrylate silicone oil in a round-bottom flask, dissolve 1.0 g of titanium oxide cluster Ti32 (R group is tert-butyl) in 10 mL of chloroform, add it to the above round-bottom flask and mix it with the terminal epoxy acrylate silicone oil. After stirring at 40°C for 5 hours, remove the chloroform by vacuum distillation, and then vacuum dry it at 60°C for 120 minutes to remove the volatiles. The obtained silicone oil is clear and transparent, and the color is consistent with the initial silicone oil. The weight is 10.87 g and the yield is 98.82%.

[0055] Example 8

[0056] Take 10 g of terminal epoxy acrylate silicone oil in a round-bottom flask, dissolve 1.0 g of titanium oxide cluster Ti32 (R group is tert-butyl) in 10 mL of chloroform, add it to the above round-bottom flask and mix it with the terminal epoxy acrylate silicone oil. After stirring at 60°C for 5 hours, remove the chloroform by vacuum distillation, and then vacuum dry it at 60°C for 120 minutes to remove the volatiles. The obtained silicone oil is clear and transparent, and the color is consistent with the initial silicone oil. The weight is 10.80 g and the yield is 98.18%.

[0057] Example 9

[0058] Take 10 g of terminal epoxy acrylate silicone oil in a round-bottom flask, dissolve 1.0 g of titanium oxide cluster Ti32 (R group is tert-butyl) in 10 mL of chloroform, add it to the above round-bottom flask and mix it with the terminal epoxy acrylate silicone oil. After stirring at 80°C for 5 hours, remove the chloroform by vacuum distillation, and then vacuum dry it at 60°C for 120 minutes to remove the volatiles. The obtained silicone oil is clear and bright, and the color is consistent with the initial silicone oil. The weight is 10.76 g and the yield is 97.82%.

[0059] Example 10

[0060] Take 10g of epoxy acrylic silicone oil into a round-bottom flask, dissolve 1.0g of titanium oxide cluster Ti32 (R group is tert-butyl) in 10mL of chloroform, add it to the above round-bottom flask and mix it with the epoxy acrylic silicone oil. After stirring at room temperature for 5h, remove the chloroform by vacuum distillation, and then vacuum dry it at 60℃ for 120min to remove the volatiles. The obtained silicone oil is clear and transparent, and the color is consistent with the initial silicone oil. The weight is 10.65g and the yield is 96.82%.

[0061] In the present invention, Figure 3 and Figure 4 The epoxy acrylic silicone oil is produced by Shandong Dayi Chemical Co., Ltd. and its model is DY-E701.

[0062] The hydrogen nuclear magnetic resonance spectra of the silicone oils obtained in Examples 1 to 4 are as follows: Figure 3 As shown. Figure 3 It can be seen that with the increase of titanium oxide clusters, the peaks of tert-butyl with a chemical shift of about 1.2 and methoxy with a chemical shift of about 3.6 in the hydrogen nuclear magnetic resonance spectrum gradually increase, indicating that the titanium oxide clusters are well combined with silicone oil.

[0063] The infrared spectra of the silicone oils obtained in Examples 1 to 4 are as follows: Figure 4 As shown. Figure 4 It can be seen that the wave number is 3010cm -1The left and right are stretching vibration peaks of unsaturated carbon-carbon double bond hydrogen, and they do not increase with the increase of the addition amount of titanium oxide clusters. In the bending vibration region, the peaks of titanium oxide cluster molecules and silicone oil overlap highly, indicating that the titanium oxide cluster molecules can be highly bonded with silicone oil.

[0064] From the above, it can be seen that the silicone oil prepared by the present invention is clear and bright, and its color is consistent with that of the initial silicone oil; the preparation method of the present invention is simple and convenient, and the yield is greater than 96%.

[0065] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing titanium oxide cluster-doped ultraviolet light-cured silicone oil, It is characterized in that The steps include: Titanium oxide cluster-doped ultraviolet light-cured silicone oil is prepared by mixing epoxy acrylic silicone oil, titanium oxide clusters and solvent.

2. The method for preparing a titanium oxide cluster-doped UV-curable silicone oil according to claim 1, It is characterized in that The usage ratio of the epoxy acrylic silicone oil, the titanium oxide cluster and the solvent is 10g:0.5-3g:1-10mL.

3. The method for preparing a titanium oxide cluster-doped UV-curable silicone oil according to claim 2, It is characterized in that The epoxy acrylate silicone oil includes terminal epoxy acrylate silicone oil and / or side epoxy acrylate silicone oil.

4. A method for preparing a titanium oxide cluster-doped UV-curable silicone oil according to claim 2 or 3, It is characterized in that The titanium oxide clusters include one or more of titanium oxide clusters Ti6, Ti8, Ti12 and Ti32.

5. The method for preparing a titanium oxide cluster-doped UV-curable silicone oil according to claim 4, It is characterized in that The titanium oxide cluster Ti6 is Ti 6 O 6 (nPrCOO) 6 (OiPr) 6 The titanium oxide cluster Ti8 is Ti 8 O 8 (tBuCOO) 16 , titanium oxide cluster Ti12 is Ti 12 O 16 (OiPr) 16 , titanium oxide cluster Ti32 is Ti32, Ti 32 (m2-O) 8 (m3-O) 8 -(OCH 2 CH 2 O) 32 (RCOO) 16 (OCH 2 CH 2 OH) 16 , wherein R = one or any combination of ethyl, propenyl, and tert-butyl.

6. The method for preparing a titanium oxide cluster-doped UV-curable silicone oil according to claim 5, It is characterized in that The solvent is chloroform.

7. The method for preparing a titanium oxide cluster-doped UV-curable silicone oil according to claim 1, It is characterized in that The mixing time is 2 to 7 hours, and the mixing temperature is 20 to 80°C.

8. Titanium oxide cluster-doped UV-curable silicone oil obtained by the method for preparing titanium oxide cluster-doped UV-curable silicone oil according to any one of claims 1 to 7.

9. Use of the titanium oxide cluster-doped UV-curable silicone oil according to claim 8 in functional elastic materials, medical dressings and packaging materials.