Anti-aging asphalt concrete anti-stripping agent and preparation method thereof
The anti-flaking agent prepared by phosphate-modified silicone solves the problems of difficulty in using acid aggregates in asphalt concrete of pumped storage power stations and poor high-temperature stability of anti-flaking agents, significantly improving the adhesion of asphalt and acidic aggregates and asphalt Hydrothermal stability of concrete.
Patent Information
- Application Number
- CN202410997022.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-12
AI Technical Summary
In the construction of asphalt concrete of pumped storage power stations, the difficulty in using acid aggregates leads to the easy peeling of asphalt. The existing anti-flaking agents have poor stability at high temperatures, making it difficult to meet construction needs.
Phosphate modified silicone is used as anti-flaking agent to prepare paste products through condensation reaction, esterification reaction and neutralization reaction, and melt and mix with petroleum asphalt to form anti-aging and anti-flaking asphalt with low melting point and oil solubility.
It significantly improves the adhesion between asphalt and acid aggregates, enhances the anti-aging performance and hydrothermal stability of asphalt concrete, and is suitable for long-term high-temperature storage and construction interruption scenarios.
Smart Images

Figure BDA0004960521480000021 
Figure BDA0004960521480000022 
Figure BDA0004960521480000023
Abstract
Description
Technical Field
[0001] The invention belongs to the field of material chemical asphalt additives, and relates to an anti-aging asphalt concrete anti-stripping agent and a preparation method thereof. The product is particularly suitable for asphalt concrete anti-seepage panels of pumped storage power stations. Background Art
[0002] Asphalt, as a building material, is widely used in the anti-seepage of pumped storage power station reservoirs and other building construction processes. Building aggregates are divided into acidic aggregates, neutral aggregates and alkaline aggregates according to the content of silica. Asphalt has good adhesion to alkaline aggregates and poor adhesion to acidic aggregates. Therefore, the application of acidic aggregates is restricted in many asphalt concrete construction projects. However, in many areas, there are no alkaline aggregates at or near the construction site of water conservancy projects. Based on local materials, only acidic aggregates, such as granite, can be used for construction projects. However, due to the strong hydrophilicity of the surface of acidic aggregates, they do not adhere firmly to oily asphalt. Under the effect of long-term water storage in the reservoir of the power station, asphalt is easily peeled off from the surface of acidic aggregates, resulting in damage to asphalt concrete buildings, which is called water damage. At present, the main way to solve this problem is to add asphalt anti-stripping agent to asphalt.
[0003] The upper and lower reservoirs of a pumped storage power station need a certain height difference, and the site selection is generally in remote mountains. Therefore, the asphalt concrete construction is significantly different from the asphalt concrete construction for ordinary roads, mainly in the following two points: First, the construction site is fixed, the asphalt concrete mixing station is close to the construction site, and a certain amount of asphalt needs to be stored at the construction site; second, the construction process of a pumped storage power station is complicated and the technology is complex, so the asphalt concrete construction is inevitably affected, and the construction is stopped for a period of time if necessary. Therefore, higher requirements are put forward for the anti-stripping agent of hydraulic asphalt concrete: good high temperature stability during a long storage time; good solubility of the anti-stripping agent in asphalt, and no stratification for long-term storage.
[0004] There are three common types of anti-stripping agents on the market. Traditional soda lime and slaked lime are used together with aggregates; amines are mainly used together with asphalt, but most amine anti-stripping agents are easily decomposed at high temperatures, and the use of amine products is limited; non-amine anti-stripping agents are miscible with asphalt, overcoming the disadvantage of amines decomposing at high temperatures. In addition to significantly improving the adhesion between asphalt and coarse aggregate, the present invention also significantly improves the anti-aging performance of asphalt due to the introduction of phosphate-modified silicone. Summary of the invention
[0005] In order to solve the above problems, the purpose of the present invention is to provide an anti-aging asphalt concrete anti-stripping agent, which can solve the problem that the asphalt concrete anti-seepage panel of the pumped storage power station is large in area and thin in thickness, and the acidic aggregate is difficult to use.
[0006] Another object of the present invention is to provide a method for preparing an anti-aging asphalt concrete anti-stripping agent.
[0007] The third object of the present invention is to provide an anti-aging and anti-stripping asphalt.
[0008] The fourth object of the present invention is to provide a method for preparing anti-stripping asphalt.
[0009] A fifth object of the present invention is to provide an application of an anti-aging asphalt concrete anti-stripping agent or anti-stripping asphalt.
[0010] In order to achieve the above object, the present invention provides an anti-aging asphalt concrete anti-stripping agent, which comprises the following raw materials by mass fraction:
[0011]
[0012] The molecular weight of the polyethylene glycol is 300 to 10000;
[0013] The alkali is one or both of potassium hydroxide and sodium hydroxide;
[0014] The catalyst is one or more of sulfuric acid, hydrochloric acid and trifluoroacetic acid.
[0015] Furthermore, the following raw materials are included by mass fraction:
[0016]
[0017] Furthermore, the rosin is one or both of disproportionated rosin and esterified rosin.
[0018] Furthermore, the structural formula of the phosphate-modified silicone is shown in the following formula (I):
[0019]
[0020] Wherein, R is polyoxyethylene or polyoxypropylene; R 1 C 1 ~C 4 Alkyl or hydrogen bond; R 2 C 1 ~C 4 Alkyl or hydrogen bond; R 3 C 1 ~C 4 Alkyl or hydrogen bond; R 4 C 1 ~C 4 Alkyl or hydrogen bond; n is an integer from 1 to 8.
[0021] Preferably, the R 1 is methyl, ethyl or propyl; R2 is methyl, ethyl, propyl, butyl or a hydrogen bond; R 3 is methyl, ethyl, propyl, butyl or a hydrogen bond; R 4 It is methyl, ethyl, propyl, butyl or hydrogen bond.
[0022] Preferably, the phosphate-modified silicone is polydimethylsiloxane PEG2 phosphate, polydimethylsiloxane PEG5 phosphate, or polydimethylsiloxane PEG7 phosphate.
[0023] Among them, PEG2 means that R is 2 connected polyoxyethylene groups, PEG5 means that R is 5 connected polyoxyethylene groups, and PEG7 means that R is 7 connected polyoxyethylene groups.
[0024] Preferably, the molecular weight of the polyethylene glycol is 500-5000.
[0025] Furthermore, the anti-stripping agent is in the form of a paste.
[0026] The present invention also provides a method for preparing the above-mentioned anti-aging asphalt concrete anti-stripping agent, comprising:
[0027] Rosin and phosphate-modified silicone are successively put into a reactor for condensation reaction, and then a catalyst and polyethylene glycol are added for esterification reaction, and then an alkali is added for neutralization reaction. The obtained product is in a paste state after cooling, and the finished asphalt concrete anti-stripping agent is obtained.
[0028] Furthermore, the condensation reaction temperature is 150°C to 180°C, and the condensation reaction time is 1 hour to 3 hours; the esterification reaction temperature is 120°C to 160°C, and the esterification reaction time is 2 hours to 3 hours; the neutralization reaction temperature is 60°C to 80°C, and the neutralization reaction time is 20 minutes to 30 minutes.
[0029] The present invention also provides an anti-stripping asphalt, comprising petroleum asphalt and the above-mentioned anti-aging asphalt concrete anti-stripping agent, which are melt-mixed to form the anti-aging anti-stripping asphalt.
[0030] Furthermore, in the anti-stripping asphalt, the amount of the anti-aging asphalt concrete anti-stripping agent accounts for 0.4% to 1.2% of the mass percentage of the anti-stripping asphalt.
[0031] The present invention also provides a method for preparing the above-mentioned anti-stripping asphalt, comprising: firstly heating and melting petroleum asphalt, adding the anti-aging asphalt concrete anti-stripping agent, stirring until the mixture is uniform, and obtaining the anti-stripping asphalt.
[0032] Furthermore, the heating and melting temperature of the petroleum asphalt is 130°C to 170°C, the stirring temperature is 130°C to 170°C, and the stirring time is 10min to 20min.
[0033] The present invention also provides the use of the anti-aging asphalt concrete anti-stripping agent or the anti-stripping asphalt in the asphalt concrete anti-seepage panel of the pumped storage power station.
[0034] The present invention has the following advantages:
[0035] 1. The anti-stripping agent of the present invention can not only significantly improve the adhesion between asphalt and acidic aggregate;
[0036] 2. The anti-stripping agent has a low melting point and good oil solubility. The product is miscible with asphalt, and the anti-stripping asphalt has good stability;
[0037] 3. The anti-stripping agent has a higher reaction temperature and good high-temperature stability, which can meet the needs of hydraulic asphalt concrete for long-term high-temperature storage due to unexpected interruptions in construction.
[0038] 4. The anti-stripping agent of the present invention can improve the anti-aging performance of asphalt concrete.
[0039] 5. The anti-stripping agent of the present invention is in a paste form and is easy to transport and store.
[0040] The beneficial effects of the present invention are:
[0041] The anti-aging asphalt anti-stripping agent provided by the present invention has obvious anti-ultraviolet aging performance, significantly enhances the adhesion between asphalt and acidic aggregate, improves the water stability and thermal stability of asphalt concrete, and can be applied to the construction of acidic aggregates for anti-seepage panels of pumped storage power stations. The asphalt anti-stripping agent provided by the present invention is simple to prepare, the conditions are easy to control, the performance is stable, and it is easy to industrialize production. DETAILED DESCRIPTION
[0042] The embodiments of the present invention will be described in detail and comprehensively below so that the advantages and features of the present invention can be more easily understood by those skilled in the art, thereby making a clearer and more definite definition of the protection scope of the present invention.
[0043] The raw materials used in the present invention are all commercially available materials.
[0044] The prepared anti-stripping agent is in the form of a yellow or brown paste at room temperature, and the color of the raw materials from different manufacturers is different.
[0045] To ensure parallel results, the same raw materials were selected for the phosphate-modified silicones.
[0046] Example 1
[0047] Add 1740g of rosin to the reactor, heat it to 180℃, and after the rosin melts, add 696g of polydimethylsiloxane PEG7 phosphate while stirring, and keep the temperature at 180℃ for two hours. After two hours, add 40g of concentrated sulfuric acid and 1536g of polyethylene glycol at a time, cool the reactor to 160℃, and keep the temperature for 3 hours, then cool it to 60℃~80℃. When the pH value of the sample test is 7, add 240g of sodium hydroxide, neutralize for 30 minutes, cool to 60℃~70℃, discharge, and cool naturally after barreling to obtain the anti-stripping agent.
[0048] Example 2
[0049] Add 1540g of rosin to the reactor, heat it to 180℃, and after the rosin melts, add 696g of polydimethylsiloxane PEG7 phosphate while stirring, and keep the temperature at 180℃ for two hours. After two hours, add 40g of concentrated sulfuric acid and 1536g of polyethylene glycol at a time, cool the reactor to 160℃, and react at the constant temperature for 3 hours, then cool to 60℃~80℃. When the pH value of the sample test is 7, add 208g of sodium hydroxide, neutralize for 30 minutes, cool to 60℃~70℃, discharge, and cool naturally after barreling to obtain the anti-stripping agent.
[0050] Example 3
[0051] Add 1940g of rosin to the reactor, heat it to 180℃, and after the rosin melts, add 696g of polydimethylsiloxane PEG7 phosphate while stirring, and keep the temperature at 180℃ for two hours. After two hours, add 40g of concentrated sulfuric acid and 1536g of polyethylene glycol at a time, cool the reactor to 160℃, and react at the constant temperature for 3 hours, then cool it to 60℃~80℃. When the pH value of the sample test is 7, add 280g of sodium hydroxide, neutralize and react for 30 minutes, cool to 60℃~70℃, discharge, and cool naturally after barreling to obtain the anti-stripping agent.
[0052] Example 4
[0053] Add 1740g of rosin to the reactor, heat it to 180℃, and after the rosin melts, add 816g of polydimethylsiloxane PEG7 phosphate while stirring, and keep the temperature at 180℃ for two hours. After two hours, add 40g of concentrated sulfuric acid and 1536g of polyethylene glycol at a time, cool the reactor to 160℃, and react at the constant temperature for 3 hours, then cool to 60℃~80℃. When the pH value of the sample test is 7, add 232g of sodium hydroxide, neutralize for 30 minutes, cool to 60℃~70℃, discharge, and cool naturally after barreling to obtain the anti-stripping agent.
[0054] Example 5
[0055] Add 1740g of rosin to the reactor, heat it to 180℃, and after the rosin melts, add 576g of polydimethylsiloxane PEG7 phosphate while stirring, and keep the temperature at 180℃ for two hours. After two hours, add 40g of concentrated sulfuric acid and 1536g of polyethylene glycol at a time, cool the reactor to 160℃, and keep the temperature for 3 hours, then cool it to 60℃~80℃. When the pH value of the sample test is 7, add 252g of sodium hydroxide, neutralize for 30 minutes, cool to 60℃~70℃, discharge, and cool naturally after barreling to obtain the anti-stripping agent.
[0056] Example 6
[0057] Add 1740g of rosin to the reactor, heat it to 180℃, and after the rosin melts, add 696g of polydimethylsiloxane PEG7 phosphate while stirring, and keep the temperature at 200℃ for two hours. After two hours, add 40g of concentrated sulfuric acid and 1536g of polyethylene glycol at a time, cool the reactor to 160℃, and react at a constant temperature for 3 hours, then cool to 60℃~80℃. When the pH value of the sample test is 7, add 240g of sodium hydroxide, neutralize for 30 minutes, cool to 60℃~70℃, discharge, and cool naturally after barreling to obtain the anti-stripping agent.
[0058] Example 7
[0059] Add 1740g of rosin to the reactor, heat it to 180℃, and after the rosin melts, add 696g of polydimethylsiloxane PEG7 phosphate while stirring, and keep the temperature at 160℃ for two hours. After two hours, add 40g of concentrated sulfuric acid and 1536g of polyethylene glycol at a time, cool the reactor to 160℃, and keep the temperature for 3 hours, then cool it to 60℃~80℃. When the pH value of the sample test is 7, add 260g of sodium hydroxide, neutralize for 30 minutes, cool to 60℃~70℃, discharge, and cool naturally after barreling to obtain the anti-stripping agent.
[0060] Example 8
[0061] Add 1740g of rosin to the reactor, heat it to 180℃, and after the rosin melts, add 696g of polydimethylsiloxane PEG7 phosphate while stirring, and keep the temperature at 180℃ for two hours. After two hours, add 40g of concentrated sulfuric acid and 1536g of polyethylene glycol at a time, cool the reactor to 180℃, and keep the temperature for 3 hours, then cool it to 60℃~80℃. When the pH value of the sample test is 7, add 240g of sodium hydroxide, neutralize for 30 minutes, cool to 60℃~70℃, discharge, and cool naturally after barreling to obtain the anti-stripping agent.
[0062] Example 9
[0063] Add 1740g of rosin to the reactor, heat it to 180℃, and after the rosin melts, add 696g of polydimethylsiloxane PEG7 phosphate while stirring, and keep the temperature at 180℃ for two hours. After two hours, add 40g of concentrated sulfuric acid and 1536g of polyethylene glycol at a time, cool the reactor to 140℃, and keep the temperature for 3 hours, then cool it to 60℃~80℃. When the pH value of the sample test is 7, add 240g of sodium hydroxide, neutralize for 30 minutes, cool to 60℃~70℃, discharge, and cool naturally after barreling to obtain the anti-stripping agent.
[0064] Example 10
[0065] Add 1740g of rosin to the reactor, heat it to 180℃, and after the rosin melts, add 696g of polydimethylsiloxane PEG7 phosphate while stirring, and keep the temperature at 180℃ for two hours. After two hours, add 40g of concentrated sulfuric acid and 1292g of polyethylene glycol at a time, cool the reactor to 160℃, and react at the constant temperature for 3 hours, then cool to 60℃~80℃. When the pH value of the sample test is 7, add 272g of sodium hydroxide, neutralize for 30 minutes, cool to 60℃~70℃, discharge, and cool naturally after barreling to obtain the anti-stripping agent.
[0066] Embodiment 11
[0067] Add 1740g of rosin to the reactor, heat it to 180℃, and after the rosin melts, add 696g of polydimethylsiloxane PEG7 phosphate while stirring, and keep the temperature at 180℃ for two hours. After two hours, add 40g of concentrated sulfuric acid and 1624g of polyethylene glycol at a time, cool the reactor to 160℃, and react at the constant temperature for 3 hours, then cool it to 60℃~80℃. When the pH value of the sample test is 7, add 228g of sodium hydroxide, neutralize for 30 minutes, cool to 60℃~70℃, discharge, and cool naturally after barreling to obtain the anti-stripping agent.
[0068] With reference to the "Adhesion Test of Coarse Aggregate and Asphalt" in the power industry standard DL / T5362 "Test Procedure for Hydraulic Asphalt Concrete", the adhesion grade of the anti-stripping agent prepared in the above embodiment was tested. Using this method to test the adhesion, the adhesion grade of common neutral and alkaline aggregates and asphalt is generally level 5, and the adhesion of asphalt and acidic aggregates mixed with anti-stripping agents is mostly level 5. Therefore, this method cannot effectively distinguish the adhesion between neutral and alkaline aggregates and asphalt. The present invention uses the time when asphalt peels off and exposes stones in the aggregate and asphalt adhesion test, that is, the initial peeling time, as a measure of the adhesion of different asphalts and aggregates. For details of the test method, see CN202110512426.5 A test method for the initial peeling time of coarse aggregate and asphalt adhesion.
[0069] The performance of the anti-stripping agent in the embodiment and the comparative example was tested, and the raw materials used in the test were:
[0070] Acidic aggregate: granite; neutral aggregate: basalt; alkaline aggregate: limestone;
[0071] Asphalt: The most commonly used 70 # Base asphalt;
[0072] Anti-stripping agent: synthetic samples of the embodiments of the present invention and comparative samples;
[0073] Anti-stripping agent dosage: expressed as a percentage of asphalt mass, the dosage is 0% or 0.6%.
[0074] The test results are shown in Tables 1 and 2. Table 1 shows the test results of the adhesion between asphalt and coarse aggregate according to DL / T5362; Table 2 shows the test results of the adhesion between asphalt and coarse aggregate when the initial peeling time is 15 minutes.
[0075] Table 1 Adhesion grade of asphalt and coarse aggregate
[0076]
[0077]
[0078] Note: "Blank asphalt" in the table is asphalt without anti-stripping agent; the amount of anti-stripping agent is 0.6%. Comparative Example 1 is an amine anti-stripping agent; Comparative Example 2 is a non-amine anti-stripping agent.
[0079] Table 2 Adhesion grade of asphalt and coarse aggregate
[0080]
[0081] Note: "Blank asphalt" in the table is asphalt without anti-stripping agent; the amount of anti-stripping agent is 0.6%. Comparative Example 1 is an amine anti-stripping agent; Comparative Example 2 is a non-amine anti-stripping agent.
[0082] Water conservancy and hydropower projects require that the adhesion of acidic aggregates used in asphalt anti-seepage panels should not be lower than that of alkaline aggregates and asphalt. According to the test method in the specification, the aggregates dipped in asphalt were slightly boiled in water for 3 minutes. The adhesion of both acidic aggregates with anti-stripping agents and alkaline aggregates without anti-stripping agents to asphalt was level 5. This method cannot effectively distinguish the effect of different anti-stripping agents on improving the adhesion between acidic aggregates and asphalt.
[0083] In Table 1, except for the asphalt without anti-stripping agent, which has a grade 2 adhesion to acidic aggregate, the others are all grade 5. Therefore, micro-boiling for 3 minutes cannot meet the working requirements of the preferred anti-stripping agent. Table 2 extends the test micro-boiling time to 15 minutes, and the effects of different anti-stripping agents can be effectively distinguished according to the asphalt shedding grade.
[0084] The sample of the embodiment of the present invention can improve the adhesion between asphalt and acidic aggregate, and can also significantly improve the water stability and thermal stability of acidic aggregate asphalt concrete.
[0085] Table 3 Effect of anti-stripping agent on long-term water stability of acid aggregate asphalt concrete
[0086]
[0087] Note: "Blank asphalt" in the table refers to asphalt without anti-stripping agent; the amount of anti-stripping agent is 0.6%.
[0088] Table 3 is a comparative test of water stability of acidic aggregates after adding anti-stripping agents, which was conducted in accordance with the "Asphalt Concrete Water Stability Test" in the power industry standard DL / T5362 "Hydraulic Asphalt Concrete Test Procedure". Since water conservancy and hydropower projects have high requirements for the application of acidic aggregates, the enhanced water stability test method used in the table extends the Marshall specimens soaking in 60°C water for 48 hours required in the specification to 128 days. The test results are shown in Table 3. This method is equivalent to the destructive effect of soaking for 100 years under natural conditions, proving that the product can meet the requirements of a century-long project of water conservancy and hydropower projects.
[0089] It can be seen from Table 3 that the compressive water stability coefficient of the anti-stripping agent increased from 0.707 when there was no anti-stripping agent to 0.967, the splitting water stability coefficient increased from 0.573 to 0.779, and the bending water stability coefficient increased from 0.275 to 0.691, which effectively improved the performance of acid aggregate asphalt concrete.
[0090] Table 4 refers to the power industry standards DL / T5362-2018, GB / T14522 and JTG E20-2011 to conduct film oven aging, UV aging and pressure heat aging tests on 70# base asphalt. The penetration of the aged asphalt was tested and compared with the penetration of the asphalt before aging to determine its aging degree and the anti-aging performance of the anti-stripping agent.
[0091] Table 4 Effect of anti-aging and anti-stripping agents on the anti-aging properties of asphalt
[0092]
[0093] Note: The dosage of anti-stripping agent is 0.6%.
[0094] In Table 4, the penetration of the asphalt after aging in three ways is significantly reduced. Among them, the film oven aging is short-term thermal aging, and the aging degree is the lightest; the pressure thermal oxygen aging is equivalent to the long-term thermal aging, and the aging degree is heavier; the ultraviolet irradiation aging is equivalent to the outdoor long-term aging, and the aging is the most serious. The asphalt mixed with the anti-aging and anti-stripping agent has the lightest aging degree among the three aging methods, especially the anti-ultraviolet aging effect is the most obvious, indicating that the anti-stripping agent of the present invention has anti-aging performance.
[0095] It can be seen from the above embodiments that the asphalt concrete anti-stripping agent provided by the present invention can effectively improve the adhesion and anti-aging properties between asphalt and aggregate, especially acidic ones, and better prevent the separation of asphalt and aggregate, thereby improving the engineering quality of asphalt concrete, extending the service life of the reservoir, and reducing the maintenance cost of the reservoir.
[0096] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the patent of the present invention. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. An anti-aging asphalt concrete anti-stripping agent, characterized by: Including the following raw materials: The molecular weight of the polyethylene glycol is 300 to 10000; The alkali is one or both of potassium hydroxide and sodium hydroxide; The catalyst is one or more of sulfuric acid, hydrochloric acid and trifluoroacetic acid.
2. The anti-aging asphalt concrete anti-stripping agent according to claim 1, characterized in that: In terms of mass fraction, it includes the following raw materials:
3. The anti-aging asphalt concrete anti-stripping agent according to claim 1 or 2, characterized in that: The rosin is one or both of disproportionated rosin and esterified rosin.
4. The anti-aging asphalt concrete anti-stripping agent according to claim 1 or 2, characterized in that: The structural formula of the phosphate-modified silicone is shown in the following formula (I): In the formula, R is one or more polyoxyethylene or polyoxypropylene groups; R1 is a C1-C4 alkyl group or a hydrogen bond; R2 is a C1-C4 alkyl group or a hydrogen bond; R3 is a C1-C4 alkyl group or a hydrogen bond; R4 is a C1-C4 alkyl group or a hydrogen bond; and n is an integer from 1 to 8.
5. The anti-aging asphalt concrete anti-stripping agent according to claim 4, characterized in that: The R1 is a methyl group, an ethyl group or a propyl group; R2 is a methyl group, an ethyl group, a propyl group, a butyl group or a hydrogen bond; R3 is a methyl group, an ethyl group, a propyl group, a butyl group or a hydrogen bond; and R4 is a methyl group, an ethyl group, a propyl group, a butyl group or a hydrogen bond.
6. The anti-aging asphalt concrete anti-stripping agent according to claim 4, characterized in that: The phosphate-modified silicone is polydimethylsiloxane PEG2 phosphate, polydimethylsiloxane PEG5 phosphate or polydimethylsiloxane PEG7 phosphate.
7. The anti-aging asphalt concrete anti-stripping agent according to claim 1 or 2, characterized in that: The molecular weight of the polyethylene glycol is 500-5000.
8. The anti-aging asphalt concrete anti-stripping agent according to claim 1 or 2, characterized in that: The anti-stripping agent is in a paste form at room temperature.
9. The method for preparing the anti-aging asphalt concrete anti-stripping agent according to any one of claims 1 to 8, characterized in that: include: Rosin and phosphate-modified silicone are successively put into a reactor for condensation reaction, and then a catalyst and polyethylene glycol are added for esterification reaction, and then an alkali is added for neutralization reaction. The obtained product is in a paste state after cooling, and the finished asphalt concrete anti-stripping agent is obtained.
10. The method for preparing the anti-aging asphalt concrete anti-stripping agent according to claim 9, characterized in that: The condensation reaction temperature is 150°C to 180°C, and the condensation reaction time is 1 hour to 3 hours; the esterification reaction temperature is 120°C to 160°C, and the esterification reaction time is 2 hours to 3 hours; the neutralization reaction temperature is 60°C to 80°C, and the neutralization reaction time is 20 minutes to 30 minutes.
11. An anti-aging and anti-stripping asphalt, characterized in that: The invention comprises petroleum asphalt and the anti-aging asphalt concrete anti-stripping agent according to any one of claims 1 to 8, and the two are melt-mixed to form anti-aging anti-stripping asphalt.
12. The anti-aging and anti-stripping asphalt according to claim 11, characterized in that: In the anti-aging and anti-stripping asphalt, the amount of the anti-aging asphalt concrete anti-stripping agent accounts for 0.4% to 1.2% of the mass percentage of the anti-stripping asphalt.
13. The method for preparing the anti-aging and anti-stripping asphalt according to claim 11 or 12, characterized in that: include: Firstly, petroleum asphalt is heated and melted, and the anti-aging asphalt concrete anti-stripping agent is added, and stirred until the mixture is uniform to obtain the anti-aging anti-stripping asphalt.
14. The method for preparing the anti-aging and anti-stripping asphalt according to claim 13, characterized in that: The heating and melting temperature of petroleum asphalt is 130℃~170℃, the stirring temperature is 130℃~170℃, and the stirring time is 10min~20min.
15. Use of the anti-aging asphalt concrete anti-stripping agent according to claims 1-8 or the anti-stripping asphalt according to claims 11-14 in asphalt concrete anti-seepage panels of pumped storage power stations.