Composite material as well as preparation method and application thereof

By using a composite material of thermogenic liquid crystal polymer, polyphenylene ether resin and polyaryletherketone resin and coupling agent modified tungsten powder, the weight change caused by traditional fish pendant is solved, and high density and low water absorption is provided Fish pendant material with good rate and corrosion resistance improves fishing effect and material stability.

CN118931224AInactive Publication Date: 2024-11-12ZHEJIANG YUANBANG MATERIAL TECH

Patent Information

Application Number
CN202411436234.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-15
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Traditional fish pendant materials have weight changes due to water absorption, which affects the fishing effect and the balance of the fishing gear, and need to be replaced regularly.

Method used

Using composite materials, including thermogenic liquid crystal polymer (LCP), polymer alloys composed of polyphenylene ether resin and polyaryletherketone resin, as well as tungsten powder modified with coupling agent, it is manufactured through a twin-screw extruder. granules, prepared fish pendant materials with high density, low water absorption and good corrosion resistance.

Benefits of technology

The fish fall has high specific gravity, low water absorption, good corrosion resistance and high impact strength, which reduces processing difficulty and improves the durability and stability of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention provides a composite material as well as a preparation method and application thereof. The composite material comprises the following raw material components in percentage by weight: 10-29% of LCP; 1-5% of a polymer alloy; 70-88% of tungsten powder modified by a coupling agent; the polymer alloy is a composite system composed of polyphenyl ether resin and polyaryletherketone resin. The composite material is high in specific gravity, good in corrosion resistance, very low in water absorption rate, not prone to loosening, good in durability and capable of being rapidly formed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer-based fish sinker preparation, and in particular to a composite material and a preparation method and application thereof. Background Art

[0002] Fish sinkers are essential auxiliary fishing tools. Their main function is to increase the weight of the fishing rig, help the hook sink and fix it in a specific water layer. However, the water absorption of fish sinkers will affect the fishing effect, mainly in the following aspects: (1) It affects the sensitivity of the float, which is very important for capturing the signal of fish biting the hook, especially when fishing for small or light-mouthed fish; (2) The weight of the fish sinker increases after absorbing water, which will change the balance of the originally adjusted fishing rig, which may cause the bait to be unstable underwater and affect the fish's baiting.

[0003] Traditional materials such as lead sinkers need to be replaced regularly due to the strong water absorption of lead. The fish sinkers made of metal tungsten powder currently on the market still have weight changes due to water absorption. Summary of the invention

[0004] In view of the above-mentioned shortcomings of the prior art, an object of the present invention is to provide a composite material and a preparation method and use thereof, so as to solve the problems in the prior art.

[0005] To achieve the above objectives and other related objectives, the present invention is achieved through the following technical solutions.

[0006] The present invention provides a composite material, comprising the following raw material components in percentage by weight: LCP 10~29%; Polymer alloy 1~5%; Tungsten powder modified by coupling agent 70~88%; The polymer alloy is a composite system composed of polyphenylene ether resin and polyaryletherketone resin.

[0007] For example, the dosage of LCP can be 10~12%, 12~14.5%, 14.5~18%, 18~20%, 20~24%, and 24~30%.

[0008] For example, the dosage of polymer alloy can be 1~1.5%, 1.5~2.0%, 2.0~2.5%, 2.5~3.0%, 3.0~3.5%, and 3.5~5%.

[0009] For example, the dosage of tungsten powder after coupling agent modification can be 70~74.5%, 74.5~82%, 82~85%, or 85~88%.

[0010] Preferably, the melting temperature of the LCP is 280°C to 350°C.

[0011] Preferably, the LCP is a thermotropic liquid crystal polymer.

[0012] More preferably, the LCP is Vectra A 950 from Celanese.

[0013] Preferably, the coupling agent is selected from one or more of dodecyltrimethoxysilane, methyltrimethoxysilane, ethyltrimethoxysilane, propyltrimethoxysilane, mercaptopropyltrimethoxysilane and vinyltriethoxysilane.

[0014] Preferably, the number average molecular weight of the polyphenylene ether resin is 25,000-35,000.

[0015] Preferably, the number average molecular weight of the polyaryletherketone resin is 25,000-35,000.

[0016] Preferably, the mass ratio of the polyphenylene ether resin to the polyaryletherketone resin is (1-1.5):1. For example, it may be 1-1.3:1 or 1.3-1.5:1.

[0017] Preferably, the particle size of the tungsten powder is 150-300 mesh, and the tungsten content is greater than 90wt%.

[0018] Preferably, the tungsten powder modified by the coupling agent is modified by soaking the tungsten powder in a coupling agent solution at 20-40° C. and pH 4-5 for 2-3 hours.

[0019] More preferably, the mass fraction of the coupling agent in the coupling agent solution is 0.3-0.5%, such as 0.3-0.4%, 0.4-0.5%.

[0020] More preferably, the coupling agent is selected from one or more of dodecyltrimethoxysilane, methyltrimethoxysilane, ethyltrimethoxysilane, propyltrimethoxysilane, mercaptopropyltrimethoxysilane and vinyltriethoxysilane.

[0021] More preferably, hydrochloric acid and / or acetic acid are used to adjust the pH of the coupling agent solution.

[0022] Preferably, the composite material comprises one or more of the following features: a) Density is 9~10g / cm 3; b) The water absorption rate is less than 0.05%; c) The sample is immersed in a 3% sodium chloride solution with a pH of 6.9 and a temperature of 45.5°C for 60 days, and the corrosion resistance grade of the sample is A; d) A 100g sample is free-fallen 100 times from a height of 5 meters, and the impact resistance grade of the sample is A~B.

[0023] More preferably, the water absorption rate of the composite material is not higher than 0.03%.

[0024] The present invention also discloses a method for preparing the composite material as described above, comprising the following steps: The tungsten powder treated with the coupling agent, the polymer alloy and the LCP are uniformly mixed and then transported to a twin-screw extruder for extrusion and granulation.

[0025] Preferably, the melting temperature is 20-30°C higher than the melting point of the LCP.

[0026] Preferably, the rotation speed of the twin-screw extruder is 80-120 r / min, and the aspect ratio is 25-32.

[0027] Preferably, the temperature of zone 1 of the twin-screw extruder is 270-275°C, the temperature of zone 2 is 280-285°C, the temperature of zone 3 is 285-290°C, the temperature of zone 4 is 290-310°C, and the temperature of zone 5 is 310-330°C.

[0028] Preferably, the particle size is 3 to 6 mm.

[0029] The present invention also provides use of the composite material as a fish sinker material.

[0030] The composite material disclosed in the present invention, as well as its preparation method and use, have the following beneficial effects: LCP, continuous basalt fiber filaments, polymer alloy and glass microbeads are compounded to make the composite material have high specific gravity, good corrosion resistance, very low water absorption rate, certain impact strength, good durability, and rapid molding; and the anisotropy caused by excessively large differences in transverse and longitudinal properties during liquid crystal polymer processing is improved, thereby reducing the processing difficulty. DETAILED DESCRIPTION

[0031] The following is a description of the implementation of the present invention by means of specific embodiments. Those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification.

[0032] Before further describing the specific embodiments of the present invention, it should be understood that the scope of protection of the present invention is not limited to the specific embodiments described below; it should also be understood that the terms used in the examples of the present invention are intended to describe specific embodiments, rather than to limit the scope of protection of the present invention. The test methods in the following examples without specifying specific conditions are generally carried out under conventional conditions or under conditions recommended by the manufacturers.

[0033] When the embodiments give numerical ranges, it should be understood that, unless otherwise specified in the present invention, both endpoints of each numerical range and any numerical value between the two endpoints can be selected. Unless otherwise defined, all technical and scientific terms used in the present invention have the same meaning as those generally understood by those skilled in the art. In addition to the specific methods, equipment, and materials used in the embodiments, according to the grasp of the prior art by those skilled in the art and the record of the present invention, any methods, equipment, and materials of the prior art similar or equivalent to the methods, equipment, and materials described in the embodiments of the present invention can also be used to realize the present invention.

[0034] The following examples of this application use the following raw materials:

[0035] The coupling agent is dodecyltrimethoxysilane.

[0036] The grade of LCP is Vectra A950 (manufacturer: Celanese Corporation), and the melting temperature is 280° C. The melting temperature is measured by DSC.

[0037] Tungsten powder was purchased from Zhuzhou Runchang New Materials Co., Ltd. with a particle size of 300 mesh and a tungsten content greater than 95wt%.

[0038] The number average molecular weight of the polyphenylene ether resin was 28,000.

[0039] The number average molecular weight of the polyaryletherketone resin is 28000. The number average molecular weight is measured by GPC.

[0040] Example 1

[0041] This embodiment provides a specific composite material, including the following raw material components in parts by weight: LCP 15%; Polymer alloy 3%; Tungsten powder after coupling agent treatment is 82%.

[0042] The polymer alloy is a composite system composed of polyphenylene ether resin and polyaryletherketone resin, and the mass ratio of the polyphenylene ether resin to the polyaryletherketone resin is 1.3:1.

[0043] The preparation method is as follows:

[0044] (1) Surface treatment of tungsten powder: soak the tungsten powder in 0.5 wt % coupling agent solution for 3 h, adjust the pH to 4, and dry at 120 ° C for 25 min.

[0045] (2) After the surface treated tungsten powder, polymer alloy and LCP are mixed evenly, they are transported to a twin-screw extruder for extrusion and granulation. The temperature of the first zone of the twin-screw extruder is 270°C, the temperature of the second zone is 280°C, the temperature of the third zone is 285°C, the temperature of the fourth zone is 290°C, and the temperature of the fifth zone is 310°C. The aspect ratio of the twin-screw extruder is 25, and the rotation speed is 100r / min.

[0046] Embodiment 2-3

[0047] This embodiment provides a specific composite material, and the contents of raw material components are shown in Table 1.

[0048] The polymer alloy is a composite system composed of polyphenylene ether resin and polyaryletherketone resin, and the mass ratio of the polyphenylene ether resin to the polyaryletherketone resin is 1.3:1.

[0049] The preparation method is the same as that in Example 1.

[0050] Example 4

[0051] This embodiment provides a specific composite material, and the contents of raw material components are shown in Table 1.

[0052] The polymer alloy is a composite system composed of polyphenylene ether resin and polyaryletherketone resin, and the mass ratio of the polyphenylene ether resin to the polyaryletherketone resin is 2.5:1.

[0053] The preparation method is the same as that in Example 1.

[0054] Comparative Example 1~2

[0055] Comparative Examples 1 and 2 are comparative examples of Example 1, except that the raw material component contents of the composite materials are different, as shown in Table 1.

[0056] In Comparative Example 1, the polymer alloy is polyphenylene ether resin; in Comparative Example 2, the polymer alloy is polyaryletherketone resin.

[0057] The preparation method is the same as that in Example 1.

[0058] Comparative Examples 3~4

[0059] Comparative Examples 3 and 4 are comparative examples of Example 1, except that the raw material component contents of the composite materials are different, as shown in Table 1.

[0060] The composition of the polymer alloy is the same as that of Example 1.

[0061] The preparation method is the same as that in Example 1.

[0062] Comparative Example 5

[0063] This comparative example is a comparative example of Example 1. The raw material component content of the composite material is the same as that of Example 1. The only difference is that the tungsten powder is not treated with a coupling agent. Other preparation processes are the same as those of Example 1.

[0064] Table 1

[0065]

[0066] The composite materials prepared in Examples 1 to 4 and Comparative Examples 1 to 5 were tested for density, corrosion resistance and water absorption. The test results are shown in Table 2. The test methods are shown below.

[0067] Density: The test is carried out in accordance with ISO1183-1-2012 "Plastics - Density determination method for non-foamed plastics - Part 1".

[0068] Corrosion resistance: The samples were immersed in a 3% by mass sodium chloride solution with a pH of 6.9 and a temperature of 45.5°C. After immersion for 60 days, the change rate of the simply supported beam notched impact strength and the change rate of the weight size of the samples were tested.

[0069] If the reduction rate of simply supported beam notched impact strength is within 5%, and the weight and size change rate is within 2%, it is grade A; if the reduction rate of simply supported beam notched impact strength is greater than 5% and less than 10%, and the weight and size change rate is greater than 2% and less than 5%, it is grade B; if the reduction rate of simply supported beam notched impact strength is not less than 10%, and the weight and size change rate is not less than 5%, it is grade C.

[0070] Water absorption rate: ASTM D570 test was adopted, the immersion temperature was 23℃, and the immersion time was 24h.

[0071] Impact resistance test: A 100g sample is dropped freely 100 times from a height of 5 meters, and visually inspected for cracks and fragments.

[0072] If no cracks are observed and no fragments are found, the impact resistance grade is A; if some of all particles have cracks but no fragments are found, the impact resistance grade is B; if some of all particles have cracks and some have fragments, the impact resistance grade is C.

[0073] Table 2

[0074]

[0075] Since the tungsten powder of Comparative Example 5 was not treated with a coupling agent, the interface compatibility of the prepared composite material was poor and powder falling occurred.

[0076] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.

Claims

1. A composite material, characterized in that: The raw material components include the following weight percentages: LCP 10~29%; Polymer alloy 1~5%; Tungsten powder modified by coupling agent 70~88%; The polymer alloy is a composite system composed of polyphenylene ether resin and polyaryletherketone resin.

2. The composite material according to claim 1, characterized in that The melting temperature of the LCP is 280° C. to 350° C.; and / or the LCP is a thermotropic liquid crystal polymer.

3. The composite material according to claim 2, characterized in that The LCP is VectraA 950 from Celanese.

4. The composite material according to claim 1, characterized in that The number average molecular weight of the polyphenylene ether resin is 25000-35000; And / or, the number average molecular weight of the polyaryletherketone resin is 25000-35000; And / or, the mass ratio of the polyphenylene ether resin to the polyaryletherketone resin is (1-1.5):1; And / or, the particle size of the tungsten powder is 150-300 mesh, and the tungsten content is greater than 90wt%.

5. The composite material according to claim 1, characterized in that The tungsten powder modified by the coupling agent is modified by soaking the tungsten powder in a coupling agent solution at 20-40° C. and pH 4-5 for 2-3 hours.

6. The composite material according to claim 5, characterized in that The mass fraction of the coupling agent in the coupling agent solution is 0.3-0.5%; And / or, the coupling agent is selected from one or more of dodecyltrimethoxysilane, methyltrimethoxysilane, ethyltrimethoxysilane, propyltrimethoxysilane, mercaptopropyltrimethoxysilane and vinyltriethoxysilane.

7. The composite material according to claim 1, characterized in that The composite material includes one or more of the following features: a) Density is 9~10g / cm 3 ; b) The water absorption rate is less than 0.05%; c) The sample is immersed in a 3% sodium chloride solution with a pH of 6.9 and a temperature of 45.5°C for 60 days, and the corrosion resistance grade of the sample is A; d) A 100g sample is free-fallen 100 times from a height of 5 meters, and the impact resistance grade of the sample is A~B.

8. A method for preparing a composite material according to any one of claims 1 to 7, characterized in that: The method comprises the following steps: uniformly mixing the tungsten powder treated with the coupling agent, the polymer alloy and the LCP, and conveying the mixture to a twin-screw extruder for extrusion and granulation.

9. The preparation method according to claim 8, characterized in that: The temperature of the first zone of the twin-screw extruder is 270-275°C, the temperature of the second zone is 280-285°C, the temperature of the third zone is 285-290°C, the temperature of the fourth zone is 290-310°C, and the temperature of the fifth zone is 310-330°C; And / or, the rotation speed of the twin-screw extruder is 80-120 r / min; And / or, the aspect ratio of the twin-screw extruder is 25-32.

10. Use of the composite material according to any one of claims 1 to 7 as a fish sinker material.

Citation Information

Patent Citations

  • Production of high-specific weight resin

    CN101074315A

  • Rapid molding high heat-resistant polyamide-polyphenyl ether alloy and preparation method thereof

    CN102876002A

  • Polyphenylene sulfide / tungsten powder shielding composite material and preparation method thereof

    CN104262963A

  • PPO / LCP / PET (Polyphenylene Oxide / Liquid Crystal Polymer / Polyethylene Terephthalate) ternary alloy material and preparation method thereof

    CN107459807A

  • Tungsten polymer fish sinker and preparation method thereof

    CN113798489A

Cited By

  • Fishing line and preparation method thereof

    CN120311378A