Building interior wall coating and preparation method thereof
Through hydrothermal treatment and inorganic acid activation of sepiolite, it forms nano nickel oxide, and carbonizes with carbon precursors at high temperature, and combines hydrolytic condensation of antibacterial monomers with silicon source, solving the problems of poor binding strength of antibacterial agents and difficulty in dispersing sepiolite. Improve the antibacterial and thermal insulation properties of building interior wall coatings.
Patent Information
- Application Number
- CN202411272269.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-11
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The poor binding force of antibacterial agents and polymer materials in existing building interior wall coatings leads to weakening of antibacterial properties. It is difficult to disperse sepiol in the paint and it is difficult to enhance the performance of composite materials.
Sepiolite is activated by hydrothermal treatment and inorganic acid, forming nano nickel oxide, and mixed with carbon precursors at high temperature to enhance the porosity and corrosion resistance of sepiolite; mixing antibacterial monomer with silicon source and passing through hydrolysis and condensation process It is coated in silicon aerogel to improve antibacterial properties.
Improve the antibacterial rate and thermal insulation properties of the coating, enhance the dispersion and adsorption properties of sepiolite, and the formed porous carbon has good thermal insulation properties, antibacterial monomers effectively inhibit microbial growth, and silicon-based aerogels are resistant. Thermal properties and mechanical strength.
Smart Images

Figure BDA0005039041750000131
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of building coatings, in particular to a building interior wall coating and a preparation method thereof. Background Art
[0002] The main type of building interior wall coating is thermal insulation coating, a functional water-based coating that blocks, reflects, and radiates near-infrared heat from the sun, insulates and cools the roof, saves energy and reduces consumption, has the characteristics of heat insulation, waterproofing, rust prevention, corrosion prevention, short construction period, and quick results, and can completely replace water sprinkler systems, thermal insulation cotton, foam sponge, sandwich iron sheets, etc. There are two main types of thermal insulation coatings based on their characteristics and principles: Isolation and conduction type: A type of coating that achieves thermal insulation through the high thermal resistance of the coating itself. It is a thick film coating. The coating is applied to a certain thickness during construction, generally 5 to 20 mm. After being fully dried and cured, the thermal conductivity of the material after drying and film formation is very small, so the coating has a certain ability to slow down the transfer of heat flow.
[0003] Antimicrobial agents are added to building interior wall paint to improve the paint's antimicrobial properties, but the bonding between polymer antimicrobial agents and paint is poor, which causes the antimicrobial agents to easily migrate and dissolve, weakening the paint's antimicrobial properties. Natural sepiolite has good thermal insulation and flame retardant properties, but sepiolite has high surface energy. When added to a paint matrix, the sepiolite fibers are glued together, making it difficult to disperse and easy to agglomerate, making it difficult to combine with polymers to enhance the performance of the composite material. Summary of the invention
[0004] The purpose of the present invention is to provide a building interior wall coating and a preparation method thereof: after the sepiolite is subjected to hydrothermal treatment and inorganic acid activation treatment, it is mixed with a nickel source and subjected to high-temperature calcination to form more uniform pores, increase the pore size and specific surface area of the sepiolite, improve the adsorption and acid and alkali corrosion resistance, form nano nickel oxide in the pores of the pretreated sepiolite, refine the pores of the pretreated sepiolite, increase the porosity of the pretreated sepiolite, and enhance the adsorption and heat resistance of the pretreated sepiolite; the sepiolite loaded with nano nickel oxide is mixed with a carbon precursor, subjected to high-temperature carbonization, and porous carbon is synthesized on the surface of the sepiolite loaded with nano nickel oxide, thereby enhancing the adsorption and heat resistance of the pretreated sepiolite. The anti-corrosion property of nickel sepiolite is combined with the porous structure of the synthesized porous carbon, which has good thermal insulation performance; the antibacterial monomer reacts with allyl bromide and is then mixed with a thiol linker to increase the molecular weight of the antibacterial monomer and avoid the migration of the antibacterial agent after washing out; the modified antibacterial monomer is mixed with a silicon source, and the modified antibacterial monomer participates in the hydrolysis reaction during the hydrolysis and condensation of the silicon source ethyl silicate, so that the modified antibacterial monomer is coated inside the silicon aerogel to avoid the small molecular weight of the antibacterial agent and easy precipitation, thereby improving the antibacterial rate of the interior wall paint, and the formed silicon-based aerogel has good heat resistance and thermal insulation performance, which improves the thermal insulation properties of the interior wall paint.
[0005] The technical problem to be solved by the present invention is as follows: adding an antibacterial agent to a building interior wall paint improves the antibacterial property of the paint, but the bonding force between the polymer antibacterial agent and the paint is poor, which causes the antibacterial agent to easily migrate and dissolve, thereby weakening the antibacterial property of the paint; natural sepiolite has good thermal insulation, flame retardancy and other properties, but the surface energy of sepiolite is high, and when added to the paint matrix, the sepiolite fibers are glued together, making it difficult to disperse and easy to agglomerate, making it difficult to combine with the polymer to enhance the performance of the composite material.
[0006] To achieve the above object, the present invention provides the following technical solutions:
[0007] A method for preparing a building interior wall coating comprises the following steps:
[0008] S1. Mixing the nano-nickel oxide-loaded sepiolite with a carbon precursor and carbonizing at high temperature to obtain a composite filler;
[0009] Furthermore, the carbon precursor is selected from one of ula grass, coconut shell, bamboo, straw, and corn starch.
[0010] More preferably, the carbon precursor is selected from one of Ula grass, coconut shell, bamboo and straw.
[0011] Further preferably, the carbon precursor is selected from Ula grass.
[0012] Furthermore, the high temperature carbonization temperature is 800-1000°C, and the carbonization time is 1-4h.
[0013] More preferably, the high temperature carbonization temperature is 800-950° C., and the carbonization time is 1-3 h.
[0014] More preferably, the high temperature carbonization temperature is 900° C. and the carbonization time is 2 h.
[0015] Furthermore, the composite filler is specifically prepared by the following steps:
[0016] The carbon precursor was rinsed three times with deionized water to remove surface soil, dried in an oven at 70°C for 12 h, taken out, cut into pieces with a length of 2 cm, placed in ethanol, stirred evenly, ethylene glycol and nano-nickel oxide-loaded sepiolite were added, stirred and reacted at 80°C for 30 min, filtered, washed with deionized water three times, dried in an oven at 90°C for 8 min, placed in a tubular furnace, activated with activator potassium hydroxide, introduced nitrogen at a flow rate of 100 mL / min, heated to 900°C, carbonized for 2 h, cooled to room temperature, taken out, washed with deionized water three times, and dried in an oven at 60°C for 10 min to obtain a composite filler.
[0017] Among them, after the carbon precursor is rinsed with deionized water three times to remove the surface soil, the shearing position is broken into pieces with a length of 2 cm, which is conducive to the carbonization of the carbon precursor Ula grass component. The treated carbon precursor Ula grass is in the organic solvent ethanol. The oxygen-containing functional groups contained in the fiber components of the Ula grass can be combined with the hydroxyl groups of ethylene glycol through chemical bonds, and the hydroxyl groups of ethylene glycol can also be combined with the hydroxyl groups contained on the surface of the nano-nickel oxide-loaded sepiolite, so that the carbon precursor Ula grass is coated on the surface of the nano-nickel oxide-loaded sepiolite;
[0018] Furthermore, the nano-nickel oxide-loaded sepiolite coated with Ula grass was carbonized at 900°C, and the potassium hydroxide molecules decomposed to form pores on the surface of the Ula grass, thereby synthesizing porous carbon on the surface of the nano-nickel oxide-loaded sepiolite, which has good thermal insulation properties, thereby improving the thermal insulation properties of the interior wall coating.
[0019] Furthermore, the ratio of the crushed segments, ethylene glycol, nano-nickel oxide-loaded sepiolite, and potassium hydroxide is (1-3) g: (0.2-0.3) g: (1.8-1.86) g: (3-7) mL.
[0020] Furthermore, the nano-nickel oxide loaded sepiolite is prepared by subjecting sepiolite to hydrothermal treatment and inorganic acid activation treatment, then mixing with a nickel source and calcining at high temperature.
[0021] Furthermore, the hydrothermal treatment temperature is 200-300°C and the time is 2-5h.
[0022] More preferably, the hydrothermal treatment temperature is 200-260° C. and the time is 2-4 h.
[0023] More preferably, the hydrothermal treatment temperature is 230° C. and the time is 3 h.
[0024] Furthermore, the inorganic acid is selected from one of hydrochloric acid, sulfuric acid and nitric acid.
[0025] More preferably, the inorganic acid is selected from hydrochloric acid and sulfuric acid.
[0026] More preferably, the inorganic acid is selected from hydrochloric acid.
[0027] Furthermore, the nickel source is selected from one of nickel nitrate, nickel sulfate, nickel chloride and nickel oxalate.
[0028] Further preferably, the nickel source is selected from nickel nitrate, nickel sulfate and nickel chloride.
[0029] Further preferably, the nickel source is selected from nickel nitrate.
[0030] Furthermore, the high temperature calcination temperature is 500-700°C and the time is 5-8h.
[0031] More preferably, the high temperature calcination temperature is 500-650° C. and the time is 5-8 h.
[0032] Preferably, the high temperature calcination temperature is 500-700°C and the time is 5-8 hours.
[0033] Furthermore, the nano-nickel oxide loaded sepiolite is prepared by the following steps:
[0034] A1. Wash the sepiolite with water, dry it in an oven at 80°C for 10 minutes, and then crush it in a pulverizer. Add the powder into deionized water, perform hydrothermal treatment at 230°C for 3 hours, filter it, wash it with deionized water three times, dry it in an oven at 60°C for 10 minutes, place it in an inorganic acid with a mass fraction of 12%, perform activation treatment for 30 minutes, heat and dehydrate it at 320°C for 2 hours, and cool it to room temperature to obtain the pretreated sepiolite.
[0035] Among them, hydrothermal treatment makes the dissociation effect of fibrous sepiolite greater than the fracture effect. Under the action of hydrothermal treatment, the fibrous sepiolite first dissociates into slender fibers and then gradually breaks to form fibrous sepiolite with a length of 1.5-5μm, which improves the dispersibility of sepiolite. After ultrafine treatment, the contact area of sepiolite with inorganic acid is increased, making it easier to dissolve magnesium ions and having better separation performance. Inorganic acid surface treatment of sepiolite, the magnesium ions in the sepiolite skeleton are replaced by hydrogen ions in inorganic hydrochloric acid, which dissolves the magnesium ions in the sepiolite, destroys the magnesium oxygen octahedral structure, reduces the filling in the silicon oxygen tetrahedral skeleton of sepiolite, and dehydrates at 320°C for 2h to remove zeolite water, bound water, and hydroxyl water from the sepiolite to form more uniform pores, increase the pore size and specific surface area of the sepiolite, and improve the adsorption and acid and alkali corrosion resistance.
[0036] Furthermore, the ratio of powder, deionized water and inorganic acid is (2-3) g:(45-55) mL:(25-35) mL.
[0037] A2. Add nickel source and citric acid to deionized water, stir until completely dissolved, add pretreated sepiolite and 36% ammonia water by mass to adjust the pH to 8.5, heat to 80°C, stir for 40 minutes, place in a 100°C oven to dry for 10 minutes, place in a Ma furnace, calcine at 600°C for 5.5 hours, and cool to room temperature to obtain nano-nickel oxide-loaded sepiolite.
[0038] The nickel precursor is mixed with citric acid and adsorbed in the pores of the pretreated sepiolite. The carboxyl group contained in the citric acid is complexed with the nickel ions to form a stable complex in the pores of the pretreated sepiolite. The citric acid is hydrolyzed to combine the nickel ions with the hydroxide ions to form nickel hydroxide in the pores of the pretreated sepiolite. The nickel hydroxide is dehydrated at a high temperature of 600°C to form nano-nickel oxide in the pores of the pretreated sepiolite, refine the pores of the pretreated sepiolite, increase the porosity of the pretreated sepiolite, enhance the thermal insulation and heat resistance of the pretreated sepiolite, and form nano-nickel oxide as a supporting skeleton of the sepiolite to prevent the dissolution of magnesium ions from the sepiolite, which causes the pores to collapse easily and affects the performance of the coating.
[0039] Furthermore, the usage ratio of nickel source, citric acid and pretreated sepiolite is (4-5) g:(4-4.2) g:(2-3) g.
[0040] S2. The modified antibacterial monomer is mixed with a silicon source to obtain a gel, the gel is placed in an aging solution for aging, and the antibacterial aerogel is obtained by washing and drying;
[0041] Furthermore, the silicon source is selected from one of ethyl orthosilicate, methyltriethoxysilane and water glass.
[0042] More preferably, the silicon source is selected from one of tetraethyl orthosilicate and water glass.
[0043] More preferably, the silicon source is selected from tetraethyl orthosilicate.
[0044] Furthermore, the aging solution is prepared by mixing ethyl orthosilicate, n-hexane and ethanol in a dosage ratio of (15-20) g:(10-15) g:(80-120) mL.
[0045] Furthermore, the specific surface area of the antibacterial aerogel is 864-874m 2 / g, pore size is 20-50nm.
[0046] Further preferably, the specific surface area of the antibacterial aerogel is 864-865m 2 / g, pore size is 20-40nm.
[0047] Further preferably, the specific surface area of the antibacterial aerogel is 864.79 m 2 / g, pore size is 30nm.
[0048] Furthermore, the antibacterial aerogel is prepared by the following steps:
[0049] The silicon source was added to ethanol and deionized water, and stirred evenly. 2 mol / L hydrochloric acid was added to adjust the pH to 2.5. The mixture was stirred at 200 r / min for 30 min, and allowed to stand for 24 to achieve sufficient hydrolysis. 2 mol / L ammonia water was added to adjust the pH to 6.5. Surface modifier hexamethyldisiloxane and modified antibacterial monomer were added, and stirred for 30 min to form a gel. The gel was washed with anhydrous ethanol for 4 times to remove unreacted water, placed in an aging solution, aged at 40°C for 20 min, washed with ethanol for 4 times to remove unreacted aging solution and impurities, and dried at 80°C for 30 min to obtain an antibacterial aerogel.
[0050] Among them, during the hydrolysis and condensation process of silicon source ethyl silicate, the mercaptopropylmethyldimethoxysilane in the modified antibacterial monomer can combine with the silicon hydroxyl group in the silicon source through chemical bonds and participate in the hydrolysis reaction, so that the modified antibacterial monomer is coated inside the silicon aerogel to avoid the antibacterial agent's small molecular weight and easy precipitation, thereby improving the antibacterial rate of the interior wall coating. In addition, the antibacterial monomer serves as the skeleton of the silicon aerogel, forming a cross-linked network structure inside the silicon aerogel, thereby improving the mechanical strength of the aerogel.
[0051] Furthermore, the usage ratio of silicon source, ethanol, deionized water, hydrochloric acid, hexamethyldisiloxane, and modified antibacterial monomer is (20-30) mL: (30-40) mL: (8-12) mL: (1-3) mL: (0.3-0.7) g: (2-3) g.
[0052] Furthermore, the modified antibacterial monomer is prepared by reacting the antibacterial monomer with allyl bromide and then mixing with a thiol linker.
[0053] Furthermore, the mercapto linker is selected from one of mercaptopropylmethyldimethoxysilane, γ-mercaptopropyltriethoxysilane, and (3-mercaptopropyl)trimethoxysilane.
[0054] More preferably, the mercapto linker is selected from one of mercaptopropylmethyldimethoxysilane and γ-mercaptopropyltriethoxysilane.
[0055] More preferably, the mercapto linker is selected from mercaptopropylmethyldimethoxysilane.
[0056] Furthermore, the antibacterial monomer is selected from one of 5,5-dimethylhydantoin, dibromohydantoin, 1-bromo-3-chloro-5,5-dimethylhydantoin and 1,3-dichloro-5,5-dimethylhydantoin.
[0057] More preferably, the antibacterial monomer is selected from 5,5-dimethylhydantoin, 1-bromo-3-chloro-5,5-dimethylhydantoin, and 1,3-dichloro-5,5-dimethylhydantoin.
[0058] More preferably, the antibacterial monomer is selected from 5,5-dimethylhydantoin.
[0059] Further, the modified antibacterial monomer is prepared by the following steps:
[0060] B1. Add antibacterial monomer and potassium hydroxide to deionized water, stir evenly, then add methanol and propylene bromide, stir until completely dissolved, place in a 60°C water bath, stir and react for 2 hours, cool to room temperature, evacuate, dry to obtain a crude product, place the crude product in 65°C petroleum ether to crystallize the crude product to obtain solid particles.
[0061] Among them, in the potassium hydroxide aqueous solution, methanol is used as a catalyst to enable one of the nitrogen-hydrogen bonds of the antibacterial monomer 5,5-dimethylhydantoin to undergo a substitution reaction with the bromine atom of allyl bromide, so that allyl bromide is grafted onto the antibacterial monomer to form 3-allyl-5,5-dimethylhydantoin, giving the reactive functional group a double bond.
[0062] Furthermore, the dosage ratio of antibacterial monomer, potassium hydroxide, deionized water, methanol and allyl bromide is (12-13) g:(5-6) g:(45-55) mL:(15-25) mL:(8-9) g.
[0063] B2. The solid particles were added to ethanol, stirred evenly, a thiol linker and dimethylphenylphosphine were added, stirred and reacted at 60°C for 30 minutes, the temperature was raised to 85°C and stirred until the organic solvent evaporated, unreacted dopants were removed by washing with deionized water, and dried in an oven at 60°C for 10 minutes to obtain a modified antibacterial monomer;
[0064] Among them, the catalyst dimethylphenylphosphine is added to the organic solvent ethanol, so that the double bond of allyl bromide in the solid particles undergoes an addition reaction with the mercapto linker mercaptopropylmethyldimethoxysilane, so that the mercapto linker mercaptopropylmethyldimethoxysilane is grafted onto the antibacterial agent monomer, thereby increasing the molecular weight of the antibacterial monomer and avoiding the migration and precipitation of the antibacterial agent.
[0065] Furthermore, the ratio of solid particles, ethanol, thiol linker, and dimethylphenylphosphine is (2-3) g: (25-35) mL: (1-1.2) g: (0.1-0.3) g.
[0066] S3. Mix the sodium silicate solution, styrene acrylic emulsion, antibacterial aerogel, composite filler and deionized water, stir evenly, add a defoamer, a dispersant and a leveling agent, stir, and obtain a building interior wall coating.
[0067] Furthermore, the sodium silicate content in the sodium silicate solution is 20-25%, the mass fraction of the styrene-acrylic emulsion is 50-55%, and the glass transition temperature is 3-7°C.
[0068] Further preferably, the sodium silicate content in the sodium silicate solution is 23.5%, the mass fraction of the styrene acrylic emulsion is 53.2%, and the glass transition temperature is 5°C.
[0069] Furthermore, the dispersant is potassium pyrophosphate or dispersant DA-4100.
[0070] Furthermore, the defoamer is selected from BYK-065 defoamer or BYK-035.
[0071] Furthermore, the leveling agent is carboxymethyl cellulose or hydroxypropyl methyl cellulose.
[0072] Compared with the prior art, the present invention has the following beneficial effects:
[0073] (1) In the technical scheme of the present invention, hydrothermal treatment is used to form fibrous sepiolite with a length of 1.5-5 μm, thereby improving the dispersibility of sepiolite. After ultrafine treatment, the contact area of sepiolite with inorganic acid is increased, making it easier to dissolve magnesium ions and having better separation performance. The sepiolite is surface treated with hydrochloric acid, and the magnesium ions in the sepiolite skeleton are replaced by hydrogen ions in inorganic hydrochloric acid, thereby dissolving magnesium ions in the sepiolite, destroying the magnesium oxygen octahedral structure, and reducing the filler in the silicon oxygen tetrahedral skeleton of the sepiolite. Dehydration at 320°C removes zeolite water and binds the sepiolite. Water and hydroxyl water form more uniform pores, increase the pore size and specific surface area of sepiolite, improve adsorption and acid and alkali corrosion resistance; form nano nickel oxide in the pores of pretreated sepiolite, refine the pores of pretreated sepiolite, improve the porosity of pretreated sepiolite, enhance the adsorption and heat resistance of pretreated sepiolite, and form nano nickel oxide with good corrosion resistance. As interior wall coating, it improves the corrosion resistance of pretreated sepiolite; in addition, nano nickel oxide is formed as the supporting skeleton of sepiolite to prevent the dissolution of magnesium ions from sepiolite, which causes the pores to collapse easily and affects the performance of the coating;
[0074] (2) In the technical scheme of the present invention, the parallel hollow vein structure of Ula grass forms a water and air circulation channel, which makes it have excellent corrosion absorption, absorb moisture, automatically adjust and maintain the degree of moisture, and can also remove odors and have warming properties. As a synthetic porous carbon material, it has good resource benefits; the carbon precursor Ula grass is coated on the surface of the nano-nickel oxide-loaded sepiolite, and after high-temperature carbonization, porous carbon is synthesized on the surface of the nano-nickel oxide-loaded sepiolite, thereby enhancing the corrosion resistance of the nano-nickel oxide-loaded sepiolite. The porous structure of the synthesized porous carbon has good thermal insulation properties, thereby improving the thermal insulation and heat preservation properties of the interior wall coating.
[0075] (3) In the technical solution of the present invention, the antibacterial monomer 5,5-dimethylhydantoin is used as an antibacterial agent to effectively inhibit the growth of microorganisms such as bacteria and molds on the surface of the coating, and effectively improve the antibacterial activity of the interior wall coating. The antibacterial monomer 5,5-dimethylhydantoin reacts with a thiol linker selected from mercaptopropylmethyldimethoxysilane through allyl bromide, so that mercaptopropylmethyldimethoxysilane is grafted on 3-allyl-5,5-dimethylhydantoin, thereby increasing the molecular weight of the antibacterial monomer and avoiding the migration of the antibacterial agent after washing out; the silicon-based ethyl silicate is hydrolyzed and condensed. During the synthesis process, the mercaptopropylmethyldimethoxysilane in the modified antibacterial monomer can combine with the silanol in the silicon source through chemical bonds and participate in the hydrolysis reaction, so that the modified antibacterial monomer is coated inside the silica aerogel to avoid the antibacterial agent's small molecular weight and easy precipitation, thereby improving the antibacterial rate of the interior wall paint. The formed silicon-based aerogel has good heat resistance and thermal insulation properties, which improves the thermal insulation properties of the interior wall paint. In addition, the antibacterial monomer serves as the skeleton of the silica aerogel, forming a cross-linked network structure inside the silica aerogel, thereby improving the mechanical strength of the aerogel. DETAILED DESCRIPTION
[0076] The technical solutions in the embodiments of the present invention are described clearly and completely. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0077] Example 1
[0078] The composite filler is prepared by the following steps:
[0079] A1. Wash 10g of sepiolite with water, dry it in an oven at 80°C for 10min, crush it in a crusher, add 2.5g of powder to 50mL of deionized water, perform hydrothermal treatment at 230°C for 3h, filter, wash with deionized water 3 times, dry it in an oven at 60°C for 10min, place it in 30mL of 12% hydrochloric acid, activate it for 30min, heat and dehydrate it at 320°C for 2h, and cool it to room temperature to obtain pretreated sepiolite;
[0080] A2. 4.5 g of nickel nitrate and 4.1 g of citric acid were added to 45 mL of deionized water and stirred until completely dissolved. 2.5 g of pretreated sepiolite and 0.5 mL of 36% ammonia were added to adjust the pH to 8.5. The mixture was heated to 80 ° C, stirred for 40 min, dried in an oven at 100 ° C for 10 min, placed in a horse furnace, calcined at 600 ° C for 5.5 h, and cooled to room temperature to obtain nano-nickel oxide-loaded sepiolite.
[0081] A3. Rinse 10g of Ula grass three times with deionized water to remove surface soil, dry it in an oven at 70°C for 12h, take it out, cut it into pieces with a length of 2cm, take 2g of the pieces and put them in 30mL of ethanol, stir evenly, add 0.25g of ethylene glycol and 1.83g of nano-nickel oxide-loaded sepiolite, stir and react at 80°C for 30min, filter, wash with deionized water three times, dry in an oven at 90°C for 8min, place it in a tube furnace, add 5mL of potassium hydroxide for activation, pass nitrogen at a flow rate of 100mL / min, heat to 900°C, carbonize for 2h, cool to room temperature, take it out, wash it with deionized water three times, and dry it in an oven at 60°C for 10min to obtain a composite filler.
[0082] Comparative Example 1
[0083] The difference between this comparative example and Example 1 is that the nano-nickel oxide-loaded sepiolite is replaced by pretreated sepiolite.
[0084] Comparative Example 2
[0085] The difference between this comparative example and Example 1 is that the carbon precursor Ula grass is not added.
[0086] Example 2
[0087] The antibacterial aerogel is prepared by the following steps:
[0088] B1. Add 12.8 g of 5,5-dimethylhydantoin and 5.6 g of potassium hydroxide to 50 mL of deionized water, stir evenly, then add 20 mL of methanol and 8.8 g of allyl bromide, stir until completely dissolved, place in a 60°C water bath, stir to react for 2 hours, cool to room temperature, evacuate, dry to obtain a crude product, place the crude product in 65°C petroleum ether to crystallize the crude product to obtain solid particles;
[0089] B2. Add 2.5 g of solid particles to 30 mL of ethanol, stir evenly, add 1.1 g of mercaptopropylmethyldimethoxysilane and 0.2 g of dimethylphenylphosphine, stir and react at 60 ° C for 30 min, heat to 85 ° C and stir until the organic solvent evaporates, wash with deionized water to remove unreacted dopants, and dry in an oven at 60 ° C for 10 min to obtain a modified antibacterial monomer;
[0090] B3. Add 25 mL of tetraethyl orthosilicate to 35 mL of ethanol and 10 mL of deionized water, stir evenly, add 2 mL of 2 mol / L hydrochloric acid to adjust the pH to 2.5, stir at 200 r / min for 30 min, let stand for 24 to achieve sufficient hydrolysis, add 2.5 mL of 2 mol / L ammonia water to adjust the pH to 6.5, add 0.5 g of hexamethyldisiloxane and 2.5 g of modified antibacterial monomer, stir for 30 min to form a gel, wash the gel with anhydrous ethanol 4 times to remove unreacted water, place it in 100 mL of aging solution, age it at 40°C for 20 min, wash it with ethanol 4 times to remove unreacted aging solution and impurities, and dry it at 80°C for 30 min to obtain antibacterial aerogel.
[0091] Comparative Example 3
[0092] The difference between this comparative example and Example 2 is that mercaptopropylmethyldimethoxysilane is not added.
[0093] Comparative Example 4
[0094] The difference between this comparative example and Example 2 is that no tetraethyl orthosilicate is added.
[0095] Example 3
[0096] A method for preparing a building interior wall coating comprises the following steps:
[0097] 25 g of 23.5% sodium silicate solution, 5 g of 53.2% styrene-acrylic emulsion, 3 g of antibacterial aerogel, 5.5 g of composite filler and 55 mL of deionized water were mixed, stirred with a high-speed dispersing homogenizer, 0.4 g of defoamer BYK-065, 0.1 g of dispersant DA-4100 and 1.3 g of carboxymethyl cellulose were added, and stirred to obtain a building interior wall coating.
[0098] Example 4
[0099] A method for preparing a building interior wall coating comprises the following steps:
[0100] 30 g of 23.5% sodium silicate solution, 7 g of 53.2% styrene-acrylic emulsion, 5 g of antibacterial aerogel, 5.8 g of composite filler and 60 mL of deionized water were mixed, stirred with a high-speed dispersing homogenizer, 0.6 g of defoamer BYK-035, 0.2 g of potassium pyrophosphate and 1.5 g of hydroxypropyl methylcellulose were added, and stirred to obtain a building interior wall coating.
[0101] Example 5
[0102] A method for preparing a building interior wall coating comprises the following steps:
[0103] 35 g of 23.5% sodium silicate solution, 9 g of 53.2% styrene-acrylic emulsion, 7 g of antibacterial aerogel, 6.1 g of composite filler and 65 mL of deionized water were mixed, stirred with a high-speed dispersing homogenizer, 0.8 g of defoamer BYK-065, 0.3 g of potassium pyrophosphate and 1.7 g of carboxymethyl cellulose were added, and stirred to obtain a building interior wall coating.
[0104] Comparative Example 5
[0105] The difference between this comparative example and Example 3 is that the composite filler is replaced by the material prepared in Comparative Example 1.
[0106] Comparative Example 6
[0107] The difference between this comparative example and Example 3 is that the composite filler is replaced by the material prepared in Comparative Example 2.
[0108] Comparative Example 7
[0109] The difference between this comparative example and Example 3 is that the antibacterial aerogel is replaced by the substance prepared in Comparative Example 3.
[0110] Comparative Example 8
[0111] The difference between this comparative example and Example 3 is that the antibacterial aerogel is replaced by the material prepared in Comparative Example 4.
[0112] The performance of the interior wall coatings prepared in Examples 3-5 and Comparative Examples 5-8 is now tested;
[0113] The thermal conductivity of the building interior wall coating was tested according to the national standard GB / T10294-2008; the antibacterial performance of the building interior wall coating prepared above was tested according to the national standard HG / T3950-2007;
[0114] The thermal insulation performance test was carried out according to the standard T / CIE082-2020 "Thermal Insulation Temperature Difference Detection Method for Thermal Insulation Coatings". The greater the temperature difference between the coating side of the sample and the back side of the sample, the more obvious the thermal insulation effect. The adhesion of the coating film was determined according to the method of GB / T9286-1998. The test results are shown in Table 1 below:
[0115] Table 1
[0116]
[0117] It can be seen from the data in Table 1 that in Comparative Example 5, the nano-nickel oxide-loaded sepiolite is replaced by pretreated sepiolite, and the prepared composite filler is added to the building interior wall paint, and its thermal insulation and corrosion resistance are reduced. This may be because the nano-nickel oxide is formed in the pores of the pretreated sepiolite to increase the porosity, enhance the adsorption performance and heat resistance, and the formed nano-nickel oxide has good corrosion resistance; Comparative Example 6 does not add the carbon precursor Ula grass, and the prepared composite filler is added to the building interior wall paint, and its thermal insulation and heat resistance are reduced. This may be because porous carbon is synthesized on the surface of the nano-nickel oxide-loaded sepiolite, which has good thermal insulation performance, thereby improving the thermal insulation and heat preservation performance of the interior wall paint; Comparative Example 7 does not add mercaptopropyl methyl dimethicone The antibacterial aerogel prepared by adding methoxysilane to the coating has a decreased antibacterial property. This may be because mercaptopropylmethyldimethoxysilane increases the molecular weight of the antibacterial monomer, avoids the migration of the antibacterial agent, participates in the hydrolysis reaction, and makes the modified antibacterial monomer coated inside the silicon aerogel, avoiding the small molecular weight of the antibacterial agent and easy precipitation; in comparative example 8, the antibacterial aerogel prepared by not adding tetraethyl orthosilicate is added to the coating, and its antibacterial and thermal insulation properties are decreased. This may be because the formed silicon-based aerogel has good heat resistance and thermal insulation properties, which improves the thermal insulation properties of the interior wall coating. In addition, the antibacterial monomer of the antibacterial aerogel as the skeleton of the silicon aerogel forms a cross-linked network structure inside the silicon aerogel, which improves the mechanical strength of the aerogel.
[0118] The data in Table 1 show that the building interior wall coatings prepared in Examples 3-5 not only have good antibacterial and heat insulation properties, but also have good adhesion and mechanical strength. The nano-nickel oxide-loaded sepiolite is mixed with a carbon precursor and carbonized at high temperature to obtain a composite filler; the modified antibacterial monomer is mixed with a silicon source to obtain a gel, and the gel is placed in an old liquid for aging, and washed and dried to obtain an antibacterial aerogel; sodium silicate solution, styrene acrylic emulsion, antibacterial aerogel, composite filler and deionized water are mixed, stirred evenly, defoamer, dispersant and leveling agent are added, stirred to obtain a building interior wall coating that meets the test performance requirements, while the building interior wall coatings prepared in Comparative Examples 5-8 do not meet the performance requirements, indicating that the building interior wall coatings prepared by the present invention not only have good antibacterial and heat insulation properties, but also have good adhesion and mechanical strength.
[0119] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0120] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. A method for preparing a building interior wall coating, characterized in that: The preparation method comprises the following steps: S1. Mixing the nano-nickel oxide-loaded sepiolite with a carbon precursor and carbonizing it at high temperature to obtain a composite filler; The nano nickel oxide loaded sepiolite is prepared by subjecting sepiolite to hydrothermal treatment and inorganic acid activation treatment, then mixing with a nickel source, and calcining at high temperature. The inorganic acid is selected from one of hydrochloric acid, sulfuric acid and nitric acid; The hydrothermal treatment temperature is 200-300°C and the time is 2-5h; The nickel source is selected from one of nickel nitrate, nickel sulfate, nickel chloride and nickel oxalate; S2. The modified antibacterial monomer is mixed with a silicon source to obtain a gel, the gel is placed in an old liquid for aging, and the antibacterial aerogel is obtained by washing and drying; The modified antibacterial monomer is prepared by reacting the antibacterial monomer with allyl bromide and then mixing with a thiol linker; The mercapto linker is selected from one of mercaptopropylmethyldimethoxysilane, γ-mercaptopropyltriethoxysilane, and (3-mercaptopropyl)trimethoxysilane; The antibacterial monomer is selected from one of 5,5-dimethylhydantoin, dibromohydantoin, 1-bromo-3-chloro-5,5-dimethylhydantoin, and 1,3-dichloro-5,5-dimethylhydantoin; S3. Mix the sodium silicate solution, styrene acrylic emulsion, antibacterial aerogel, composite filler and deionized water, stir evenly, add a defoamer, a dispersant and a leveling agent, stir, and obtain a building interior wall coating.
2. The method for preparing a building interior wall coating according to claim 1, characterized in that: The carbon precursor is selected from one of ula grass, coconut shell, bamboo, straw and corn starch.
3. The method for preparing a building interior wall coating according to claim 1, characterized in that: The high temperature carbonization temperature is 800-1000° C., and the carbonization time is 1-4 hours.
4. The method for preparing a building interior wall coating according to claim 1, characterized in that: The silicon source is selected from one of ethyl orthosilicate, methyltriethoxysilane and water glass.
5. The method for preparing a building interior wall coating according to claim 1, characterized in that: The aging solution is composed of ethyl orthosilicate, n-hexane and ethanol according to The mixture is mixed in a dosage ratio of (15-20) g:(10-15) g:(80-120) mL.
6. The method for preparing a building interior wall coating according to claim 1, characterized in that: The specific surface area of the antibacterial aerogel is 864-874m 2 / g, pore size is 20-50nm.
7. The method for preparing a building interior wall coating according to claim 1, characterized in that: The antibacterial monomer is selected from one of 5,5-dimethylhydantoin, 1-bromo-3-chloro-5,5-dimethylhydantoin and 1,3-dichloro-5,5-dimethylhydantoin.
8. The method for preparing a building interior wall coating according to claim 1, characterized in that: The sodium silicate content in the sodium silicate solution is 20-25%; the mass fraction of the styrene-acrylic emulsion is 50-55%, and the glass transition temperature is 3-7°C.
9. The method for preparing a building interior wall coating according to claim 1, characterized in that: The dispersant is potassium pyrophosphate or dispersant DA-4100; the defoamer is selected from defoamer BYK-065 or defoamer BYK-035; and the leveling agent is carboxymethyl cellulose or hydroxypropyl methyl cellulose.
10. A building interior wall coating prepared according to the preparation method according to any one of claims 1 to 9.