Porous graphene microsphere-based ultra-black coating as well as preparation method and application thereof

Through the preparation method of porous graphene microsphere-based ultra-black coating, the problem of complex time-consuming preparation of ultra-black materials and insufficient ultraviolet light absorption is solved, and efficient and simple preparation of ultra-black coatings is achieved, with more than 99% light Absorption performance, suitable for the fields of anti-ice and optical regulation.

CN118931269AActive Publication Date: 2024-11-12SICHUAN UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411208987.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-11-12
Estimated Expiration
2044-08-30

AI Technical Summary

Technical Problem

The existing ultra-black materials are complex and time-consuming, and it is difficult to meet the needs of large-scale applications. Most methods lack ultraviolet light absorption performance. The smooth surface microsphere structure leads to a high reflectivity of incident light, which limits its application.

Method used

Using the preparation method of porous graphene microsphere-based ultra-black coating, graphene and 1-pyrene ester cyclodextrin are ultrasonic dispersed in aqueous sodium hydroxide solution to form a microsphere precursor solution and in an ethyl acetate ice bath Ice, then the microspheres are filtered and freeze-dried to form a porous structure, which is dispersed in the resin solution to spray to form an ultra-black coating with high light absorption properties.

Benefits of technology

It has achieved a high incident light absorption rate, especially the ultraviolet light absorption rate, and the coating can achieve light absorption performance of more than 99%, and simplified the preparation process. It is suitable for large-scale production and is suitable for anti-ice and optical regulation fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118931269A_ABST
    Figure CN118931269A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and application of a porous graphene microsphere-based ultra-black coating. The preparation method comprises the following steps: (1) ultrasonically dispersing graphene in deionized water to obtain a dispersion liquid of graphene in water, dissolving 1-pyrene cyclodextrin (Py-CD) in a sodium hydroxide aqueous solution, adding the Py-CD aqueous solution into the dispersion liquid, performing ultrasonic treatment to obtain a microsphere precursor solution, and drying the microsphere precursor solution to obtain a porous graphene microsphere-based ultra-black coating; spraying the microsphere precursor solution into an organic solvent of ethyl acetate ice bath, filtering to obtain ice balls, and freeze-drying to obtain graphene / Py-CD microspheres with a porous structure; (2) preparing a resin solution, and dispersing the obtained porous graphene / Py-CD microspheres in the resin solution to obtain a spraying precursor solution; and (3) spraying the precursor solution onto the surface of a material, and drying to obtain the porous graphene microsphere-based ultra-black coating. The ultra-black coating has high incident light absorptivity and has application value in preparation of materials with high light absorption performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of light-absorbing materials, and in particular to a porous graphene microsphere-based ultra-black coating and a preparation method and application thereof. Background Art

[0002] Ultra-black materials have attracted much attention due to their low surface reflectivity and excellent light absorption performance in a wide range of incident light. Ultra-black materials have been applied in many fields of optical regulation, such as infrared stealth, stray light regulation, solar energy collection, etc. The ideal ultra-black material needs to absorb almost all incident light in a wide range of wavelengths, because a material with a 1% light absorption difference will result in a difference of at least one order of magnitude in the suppression level of stray light (Opt. Express 2017, 25, 26175–26185). This shows that it is very important to prepare materials with high light absorption performance.

[0003] The light absorption properties of ultra-black materials mainly depend on their structure and light-absorbing medium. Carbon materials such as graphene, carbon nanotubes, and carbon black have a wider range of light absorption properties in ultra-black material applications due to their relatively large conjugated system and moderate free electron density. In the past few decades, there have been many applications of carbon materials in ultra-black materials, such as the single-walled carbon nanotube forest with multiple scattering characteristics prepared by chemical vapor deposition (Nano Lett. 2008, 8, 446-451), which is the ultra-black material with the lowest reflectivity reported so far. It also provides new ideas for the design of ultra-black materials, namely: by adjusting the micromorphology of carbon materials to form micro-nano light capture structures to achieve ideal light absorption properties. In order to realize the design of the microstructure of ultra-black materials, vapor deposition, chemical etching (Adv. Energ. Sust. Res. 2021, 2 (4), 2000083), laser processing and other methods are usually used.

[0004] Although the preparation methods of ultra-black materials have developed rapidly in the past few decades, ultra-black materials still face many challenges in actual large-scale applications. Most methods for producing ultra-black materials require sophisticated instruments or complex preparation processes (Chem. Eng. J. 2023, 466, 143067) (ACS Appl. Mater. Inter. 2023, 15, 11369-11378). The production process not only requires harsh conditions of high temperature or vacuum, but also takes a long time, which cannot meet the requirements of large-scale application of materials in practical applications. For example, single-walled carbon nanotube forests need to grow at a high temperature of 450°C, and the preparation process is complicated and time-consuming. This type of method greatly limits the scale-up capability and actual application of ultra-black materials. The use of spraying to prepare ultra-black coatings can quickly and efficiently prepare ultra-black materials, which is very promising in the large-scale production of ultra-black materials. Huiyong Li (ACS Appl. Mater. Inter. 2023, 15, 11369-11378) et al. used a magnetic field-assisted spraying method to prepare an ultra-black material with a needle-shaped array structure. Although the spraying method can quickly prepare the ultra-black coating, the introduction of the magnetic field during the preparation process still limits its large-scale preparation, and when preparing ultra-black materials with complex surfaces, the limitation of the magnetic field is more obvious; Yuefan Hu (ACS Appl. Nano Mater. 2021, 4, 7995-8002) et al. prepared hollow carbon spheres by a silica template method, and used hollow carbon spheres to prepare ultra-black coatings by spraying, achieving a more convenient ultra-black coating preparation. However, it is worth noting that the smooth microsphere structure may still cause the incident light to produce a higher interface reflection when it contacts the surface of the carbon sphere, resulting in a reduction in the absorption rate of the incident light. In addition, the current ultra-black coating basically only focuses on the absorption of visible light, and does not involve the absorption of ultraviolet light. Summary of the invention

[0005] The purpose of the present invention is to provide a porous graphene microsphere-based ultra-black coating and a preparation method thereof. The coating has a high incident light absorptivity and has application value in preparing materials with high light absorption performance.

[0006] In order to achieve the above object, the present invention provides a method for preparing a porous graphene microsphere-based ultra-black coating, comprising the following steps:

[0007] (1) preparing graphene into a dispersion, dissolving 1-pyrene ester cyclodextrin in a sodium hydroxide aqueous solution and adding the resulting solution to the dispersion, ultrasonically obtaining a microsphere precursor, spraying the microsphere precursor into an organic solvent in an ethyl acetate ice bath, ensuring that the aqueous dispersion can immediately freeze to form microspheres when in contact with the organic solvent, filtering the collected microspheres and freeze-drying them to obtain graphene / Py-CD microspheres having a porous structure;

[0008] (2) preparing a resin solution, dispersing the obtained porous graphene / Py-CD microspheres in the resin solution to obtain a spraying precursor solution;

[0009] (3) Spraying the obtained spraying precursor liquid onto the surface of the material, and obtaining a porous graphene microsphere-based ultra-black coating after drying.

[0010] Preferably, in the above step (1), the dispersion is obtained by dispersing graphene in deionized water; the concentration of the sodium hydroxide aqueous solution is 0.1M; the spraying is performed using an air spray gun, the nozzle diameter is 0.3mm-0.8mm, and the working air pressure is 1.5-4bar; the organic solvent is an organic solvent having a melting point lower than that of ethyl acetate and being immiscible with water, preferably selected from n-hexane, diethyl ether or 2-methylpentane; and the freeze-drying temperature is -80 degrees Celsius.

[0011] Preferably, in the microsphere precursor solution in the above step (1), the final concentration of graphene is 2-6 mg / mL, the final concentration of 1-pyrene ester cyclodextrin is 0.1-2 mg / mL, and the particle size of the obtained graphene / Py-CD microspheres is 1-100 μm.

[0012] Preferably, the resin solution in the above step (2) may be selected from any one of polydimethylsiloxane, polychlorotrifluoroethylene-vinylidene fluoride copolymer, polychlorotrifluoroethylene, polyvinylidene chloride, and polymethyl methacrylate, and the solvent for dissolving the resin may be selected from any one of acetone, ethanol, ethylene dichloride, n-hexane, tetrahydrofuran, cyclohexane, and dichloromethane.

[0013] Preferably, the concentration of the resin in the resin solution in the above step (2) is 1wt% to 10wt%; and the mass ratio of the resin to the porous graphene / Py-CD microspheres in the spraying precursor solution is 1:1 to 20:1.

[0014] Preferably, the spraying in the above step (3) is performed using an air spray gun, the nozzle diameter of which is 0.3 mm to 0.8 mm and the working pressure is 1.5 to 4 bar.

[0015] Preferably, the material in the above step (3) can be selected from aluminum plates, glass, paper sheets, rubber, plastics and other materials that can be used for spraying.

[0016] Preferably, the thickness of the coating obtained in the above preparation method is 50 μm to 300 μm.

[0017] The present invention also provides an ultra-black coating prepared by the above-mentioned preparation method. The ultra-black coating can be applied to the field of anti-icing, and the coating has a significant ability to delay icing.

[0018] The ultra-black coating provided by the present invention can also be used to prepare materials with light absorption performance. The light absorption performance of the material coated with the coating is significantly improved, and the incident light absorption can reach more than 99%.

[0019] The ultra-black coating and preparation method thereof provided by the present invention have the following advantages:

[0020] The present invention provides a porous graphene-based microsphere for preparing an ultra-black coating. Since the graphene microsphere contains a large number of nanopore structures, these porous structures and the micrometer gaps between the microspheres together form a micro-nano light capture structure. In particular, when the incident light contacts the surface of the porous microsphere, the light will further enter the interior of the microsphere through the holes on the surface of the microsphere, and reduce the interface reflection based on the Fresnel law. The incident light entering the interior of the microsphere will be reflected multiple times inside the microsphere and finally absorbed, thereby achieving a high incident light absorption rate. In addition, since cyclodextrin pyrene ester can be assembled on graphene through π-π interaction to form a large conjugated structure, this large conjugated structure is very conducive to the absorption of ultraviolet light.

[0021] The present invention adopts a simple, fast and efficient direct spraying method to prepare the ultra-black coating. Compared with other preparation methods, the preparation process is simple, no additional complex equipment is required, the preparation conditions are mild, no harsh environmental conditions are required, the time is short, and it is conducive to large-scale production. Compared with other spraying methods, there are no additional conditions during the spraying process, the preparation time is short, a large amount of ultra-black coating can be obtained in a short time, and it can absorb more than 99% of the incident light, which has significant application value in the preparation of materials with high light absorption performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is the electron microscope scanning result of the porous graphene microspheres obtained in Example 1 of the present invention.

[0023] Figure 2 This is the effect of spraying the ultra-black coating on the mask according to Example 2 of the present invention.

[0024] Figure 3 The anti-icing test results of the coating obtained in Example 5 of the present invention are shown.

[0025] Figure 4 These are the UV-visible-near-infrared reflection spectrum results of the porous graphene@resin coatings obtained in Examples 1 to 6 of the present invention.

[0026] Figure 5 The anti-icing test results of the coating obtained in Example 6 of the present invention are shown. DETAILED DESCRIPTION

[0027] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0028] Note: The experimental methods in the following examples are conventional methods unless otherwise specified, and are performed according to the techniques or conditions described in the literature in the field or according to the product instructions. The materials, reagents, etc. used in the following examples are all commercially available unless otherwise specified.

[0029] Example 1

[0030] This embodiment provides a method for preparing a porous graphene microsphere-based ultra-black coating, which is as follows:

[0031] (1) Preparation of porous graphene / Py-CD microspheres:

[0032] 3 g of graphene was ultrasonically dispersed in 500 mL of deionized water and placed in a 1000 mL beaker, and ultrasonically dispersed for 3 h to obtain a dispersion of graphene in water; 500 mg of 1-pyrene ester cyclodextrin (Py-CD) was dissolved in 20 mL of 0.1 M sodium hydroxide aqueous solution, and then the Py-CD aqueous solution was added to the graphene aqueous dispersion, and ultrasonic treatment was performed to obtain a microsphere precursor solution, and the microsphere precursor solution was loaded into a container matching an air spray gun, and the working pressure of the air spray gun was adjusted to 3 bar, and 900 mL of ether treated with 500 mL of ethyl acetate in an ice bath was used to collect the sprayed droplets, and the collected microspheres were filtered through a metal filter and freeze-dried to obtain graphene / Py-CD microspheres with a particle size of 1 to 100 μm.

[0033] (2) Preparation of porous graphene / Py-CD microsphere resin dispersion:

[0034] The polychlorotrifluoroethylene-vinylidene fluoride copolymer was dissolved in acetone to obtain a resin solution, and the final solution concentration was set to 8.38wt%. 30mg of porous graphene microspheres were dispersed in the resin solution by ultrasonication for 15min, and the mass of resin in the dispersion: the mass of porous graphene microspheres = 20:1, wherein the resin will be wrapped on the surface of the microspheres to form a resin dispersion of the microspheres.

[0035] (3) Preparation of porous graphene / Py-CD@resin ultra-black coating:

[0036] The resin dispersion with porous graphene microspheres is placed in an air spray gun with a needle diameter of 0.5 mm. An air pump is used to pressurize the gun and the pressure is set to 3 bar. The resin dispersion is sprayed on an aluminum plate. Since the acetone in the dispersion has a low boiling point, it will evaporate rapidly during the spraying process, and the polymer resin is wrapped on the surface of the porous graphene microspheres. After the solution evaporates, the resin can provide good adhesion to the substrate, and finally an ultra-black coating is obtained.

[0037] The obtained ultra-black coating was scanned by electron microscope, and the results were as follows: Figure 1 As shown in the figure, it can be seen that the particle size of the microspheres in the coating is between 20 μm and 70 μm, and the microspheres have a porous surface structure, which is conducive to the incident light further entering the interior of the microspheres and being further absorbed.

[0038] Example 2

[0039] This embodiment provides a method for preparing an ultra-black coating, which is as follows:

[0040] (1) Preparation of porous graphene / Py-CD microspheres:

[0041] 2 g of graphene was ultrasonically dispersed in 500 mL of deionized water and placed in a 1000 mL beaker, and ultrasonically dispersed for 2 h to obtain a dispersion of graphene in water; 100 mg of 1-pyrene ester cyclodextrin (Py-CD) was dissolved in 20 mL of 0.1 M sodium hydroxide aqueous solution, and then the Py-CD aqueous solution was added to the graphene aqueous dispersion, and ultrasonic treatment was performed to obtain a microsphere precursor solution, and the precursor solution was loaded into a container matching an air spray gun, and the working pressure of the air spray gun was adjusted to 4 bar, and 900 mL of n-hexane treated with 500 mL of ethyl acetate in an ice bath was used to collect the obtained droplets, and the collected microspheres were filtered through a metal filter and freeze-dried to obtain graphene / Py-CD microspheres with a particle size of 1 to 100 μm.

[0042] (2) Preparation of porous graphene / Py-CD microsphere resin dispersion:

[0043] Polymethyl methacrylate was dissolved in dichloroethane to obtain a resin solution with a final solution concentration of 3wt%. 30mg of porous graphene microspheres were dispersed in the resin solution by ultrasonic method. The mass of resin in the dispersion: the mass of porous graphene microspheres = 5:1. The resin was wrapped on the surface of the microspheres to form a resin dispersion of the microspheres.

[0044] (3) Preparation of porous graphene / Py-CD@resin ultra-black coating:

[0045] The resin dispersion with porous graphene microspheres is placed in an air spray gun with a needle diameter of 0.5 mm. An air pump is used to pressurize the resin dispersion and the pressure is set to 1.5 bar. Since the acetone in the dispersion has a low boiling point, it will evaporate rapidly during the spraying process, and the polymer resin is wrapped on the surface of the porous graphene microspheres. After the solution evaporates, the resin can provide good adhesion to the substrate, and finally an ultra-black coating is obtained.

[0046] Under the same conditions, the microsphere resin dispersion was directly sprayed on a white mask to observe the light absorption capacity of the coating. The coating thickness was about 200 μm. The results are as follows Figure 2 As shown, it can be seen that before spraying, the white mask ( Figure 2 Left) A "nose" with a three-dimensional geometric shape, after spraying, photo ( Figure 2 Right) presents a two-dimensional planar shape, a phenomenon that shows that the ultra-black coating has excellent light absorption properties.

[0047] Example 3

[0048] This embodiment provides a method for preparing an ultra-black coating, which is as follows:

[0049] (1) Preparation of porous graphene / Py-CD microspheres:

[0050] 3 g of graphene was ultrasonically dispersed in 800 mL of deionized water and placed in a 1000 mL beaker, and ultrasonically dispersed for 2 h to obtain a dispersion of graphene in water; 400 mg of 1-pyrene ester cyclodextrin (Py-CD) was dissolved in 20 mL of 0.1 M sodium hydroxide aqueous solution, and then the Py-CD aqueous solution was added to the graphene aqueous dispersion, and ultrasonic treatment was performed to obtain a microsphere precursor solution, and the precursor solution was loaded into a container matching an air spray gun, and the working pressure of the air spray gun was adjusted to 2 bar, and 900 mL of n-hexane treated with 500 mL of ethyl acetate in an ice bath was used to collect the obtained droplets, and the collected microspheres were filtered through a metal filter and freeze-dried to obtain graphene / Py-CD microspheres with a particle size of 1 to 100 μm.

[0051] (2) Preparation of porous graphene / Py-CD microsphere resin dispersion:

[0052] 30 mg of porous graphene microspheres were directly dispersed in an acetone solution by ultrasonic method to obtain a microsphere dispersion, in which the mass of resin in the dispersion: the mass of porous graphene microspheres = 0:1.

[0053] (3) Preparation of porous graphene / Py-CD@resin ultra-black coating:

[0054] The acetone dispersion containing porous graphene microspheres is placed in an air spray gun with a needle diameter of 0.5 mm. An air pump is used to pressurize the dispersion, and the pressure is set to 2 bar to spray the dispersion onto an aluminum plate. Since the acetone dispersion has a low boiling point, it will evaporate rapidly during the spraying process. Since no resin is added as an adhesive, the adhesion performance to the aluminum plate substrate is poor.

[0055] Example 4

[0056] This embodiment provides a method for preparing an ultra-black coating, which is as follows:

[0057] (1) Preparation of porous graphene / Py-CD microspheres:

[0058] 3 g of graphene was ultrasonically dispersed in 400 mL of deionized water and placed in a 1000 mL beaker, and ultrasonically dispersed for 2 h to obtain a dispersion of graphene in water; 450 mg of 1-pyrene ester cyclodextrin (Py-CD) was dissolved in 20 mL of 0.1 M sodium hydroxide aqueous solution, and then the Py-CD aqueous solution was added to the graphene aqueous dispersion, and ultrasonic treatment was performed to obtain a microsphere precursor solution, which was loaded into a container supporting an air spray gun, and the working pressure of the air spray gun was adjusted to 3 bar. 900 mL of 2-methylpentane treated with 900 mL of ethyl acetate in an ice bath was used to collect the obtained droplets, and the collected microspheres were filtered through a metal filter and freeze-dried to obtain graphene microspheres.

[0059] (2) Preparation of porous graphene / Py-CD microsphere resin dispersion:

[0060] Dissolve polydimethylsiloxane in ethanol to obtain a resin solution with a final solution concentration of 1 wt%. Take 30 mg of porous graphene / Py-CD microspheres and disperse them in the resin solution by ultrasonic method. The mass of resin in the dispersion: the mass of porous graphene microspheres = 1:1, wherein the resin will be wrapped on the surface of the microspheres to form a resin dispersion of the microspheres.

[0061] (3) Preparation of porous graphene / Py-CD@resin ultra-black coating:

[0062] The resin dispersion with porous graphene microspheres is placed in an air spray gun. Larger microsphere particle sizes require a larger needle diameter for the air spray gun. The needle diameter of the spray gun used is 0.8 mm. An air pump is used to pressurize the pressure, and the pressure is set to 3 bar. The dispersion is sprayed on a piece of paper. Since the acetone in the dispersion has a low boiling point, it will evaporate rapidly during the spraying process, and the polymer resin is wrapped around the surface of the porous graphene microspheres. After the solution evaporates, the resin can provide good adhesion to the substrate, and finally an ultra-black coating is obtained.

[0063] Example 5

[0064] This embodiment provides a method for preparing an ultra-black coating and an application thereof, as follows:

[0065] (1) Preparation of porous graphene / Py-CD microspheres:

[0066] 3 g of graphene was ultrasonically dispersed in 500 mL of deionized water and placed in a 1000 mL beaker, and ultrasonically dispersed for 3 h to obtain a dispersion of graphene in water; 500 mg of 1-pyrene ester cyclodextrin (Py-CD) was dissolved in 20 mL of 0.1 M sodium hydroxide aqueous solution, and then the Py-CD aqueous solution was added to the graphene aqueous dispersion, and ultrasonic treatment was performed to obtain a microsphere precursor solution, which was loaded into a container supporting an air spray gun, and the working pressure of the air spray gun was adjusted to 2.5 bar. The droplets were collected in 900 mL of n-hexane treated with 500 mL of ethyl acetate in an ice bath, and the collected microspheres were filtered through a metal filter and freeze-dried to obtain graphene / Py-CD microspheres with a particle size of 1 to 100 μm.

[0067] (2) Preparation of porous graphene / Py-CD microsphere resin dispersion:

[0068] The polychlorotrifluoroethylene-vinylidene fluoride copolymer was dissolved in acetone to obtain a resin solution with a final solution concentration of 2wt%. 30mg of graphene microspheres were dispersed in the resin solution by ultrasonic method. The mass of resin in the dispersion: the mass of porous graphene microspheres = 3:1, wherein the resin will be wrapped on the surface of the microspheres to form a resin dispersion of the microspheres.

[0069] (3) Preparation of porous graphene / Py-CD@resin ultra-black coating:

[0070] The resin dispersion with porous graphene microspheres is placed in an air spray gun. Larger microsphere particle sizes require a larger needle diameter for the air spray gun. The needle diameter of the spray gun used is 0.5 mm. An air pump is used to pressurize the dispersion, and the pressure is set to 2.5 bar to spray the dispersion onto an aluminum plate. Since the acetone in the dispersion has a low boiling point, it will evaporate rapidly during the spraying process, and the polymer resin is wrapped around the surface of the porous graphene microspheres. After the solution evaporates, the resin can provide good adhesion to the substrate, and finally an ultra-black coating is obtained.

[0071] The obtained coating was placed on a cold stage at -20°C, and 50 μL of deionized water was dripped on the coating to characterize the anti-icing performance of the coating. The same steps were performed on an unsprayed aluminum plate as a control experiment, and the results were as follows: Figure 3 As shown in the figure, the white substrate is an aluminum plate, and the black substrate is an aluminum plate sprayed with a coating. It can be seen that the water droplets on the aluminum plate ( Figure 3 White substrate) completely freezes within 60s, while water droplets on the coating ( Figure 3The black substrate) did not freeze at 90s. The coating had a significant ability to delay freezing compared to the uncoated aluminum plate.

[0072] Example 6

[0073] This embodiment also provides a method for preparing an ultra-black coating and an application thereof, as follows:

[0074] (1) Preparation of porous graphene / Py-CD microspheres:

[0075] 1.2 g of graphene was ultrasonically dispersed in 200 mL of deionized water and placed in a 1000 mL beaker. The dispersion was ultrasonically dispersed for 3 h to obtain a dispersion of graphene in water. 500 mg of 1-pyrene ester cyclodextrin (Py-CD) was dissolved in 20 mL of 0.1 M sodium hydroxide aqueous solution. The Py-CD aqueous solution was then added to the graphene aqueous dispersion and ultrasonically treated to obtain a microsphere precursor solution. The precursor solution was loaded into a container equipped with an air spray gun, and the working pressure of the air spray gun was adjusted to 3 bar. The droplets were collected using 500 mL of n-hexane treated with 500 mL of ethyl acetate in an ice bath. The collected microspheres were filtered using a metal filter and freeze-dried to obtain graphene / Py-CD microspheres with a particle size of 1 to 100 μm.

[0076] (2) Preparation of porous graphene / Py-CD microsphere resin dispersion:

[0077] The polychlorotrifluoroethylene-vinylidene fluoride copolymer was dissolved in acetone to obtain a resin solution with a final solution concentration of 1wt%. 25mg of porous graphene microspheres were dispersed in the resin solution by ultrasonic method. The mass of resin in the dispersion: the mass of porous graphene microspheres = 2:1, wherein the resin will be wrapped on the surface of the microspheres to form a resin dispersion of the microspheres.

[0078] (3) Preparation of porous graphene / Py-CD@resin ultra-black coating:

[0079] The resin dispersion with porous graphene microspheres is placed in an air spray gun. Larger microsphere particle sizes require a larger needle diameter for the air spray gun. The needle diameter of the spray gun used is 0.5 mm. An air pump is used to pressurize the dispersion, and the pressure is set to 3 bar to spray the dispersion onto an aluminum plate. Since the acetone in the dispersion has a low boiling point, it will evaporate rapidly during the spraying process, and the polymer resin is wrapped around the surface of the porous graphene microspheres. After the solution evaporates, the resin can provide good adhesion to the substrate, and finally an ultra-black coating is obtained.

[0080] The resin in the above preparation method can also be selected from polymer resins such as polytrifluorochloroethylene and polyvinylidene chloride; the solvent for dissolving the resin can also be selected from solvents such as n-hexane, tetrahydrofuran, cyclohexane, and dichloromethane; the above spraying material can also be selected from rubber or plastic.

[0081] In order to simulate the freezing behavior of the coating under natural conditions, the obtained coating was placed on a cold table at a temperature of -15°C, a xenon lamp was used to simulate sunlight in a natural environment, the light intensity was set to 1 sun intensity, and the cold table was tilted 15°. An aluminum plate without spray coating was used as a control sample. After the aluminum plate and the coating were placed on the cold table for 1 minute, 20 mL of supercooled water (water in this supercooled state can easily freeze under slight stimulation such as shaking) that had been frozen in a -18°C refrigerator for 3 hours was added dropwise, and the freezing of the control aluminum plate and the coating was observed. The results are as follows: Figure 4 As shown, Figure a is the process diagram of the control sample aluminum plate anti-icing experiment, Figure b is the result diagram of the control sample aluminum plate anti-icing experiment; Figure c is the process diagram of the coating anti-icing experiment, and Figure d is the result diagram of the coating anti-icing experiment. Figure 4 It can be seen that after being treated with supercooled water, a layer of ice ( Figure 4 b), and the coating did not freeze ( Figure 4 d), which shows that the coating provided by the present invention has excellent anti-icing ability in practical applications.

[0082] The ultra-black coatings obtained in Examples 1 to 6 were tested for reflectivity against ultraviolet, visible, and near-infrared light, and the results were as follows: Figure 5 As shown, it can be seen that, except for Example 1, the light reflectivity of the coatings prepared in the other examples in the near-infrared region is less than 1%, indicating that the absorption of this part of the incident light reaches more than 99%, and the average reflectivity of the coatings obtained in Examples 2, 5, and 6 from the ultraviolet to the near-infrared region is less than 1%, indicating that the average absorption of the incident light by the coating reaches more than 99%. It can be seen that the ultra-black coating obtained by the preparation method provided in the embodiment of the present invention has efficient light absorption performance, and the coating can be used to prepare materials with efficient light absorption performance. The coating and the prepared materials have great application potential in the field of light absorption.

[0083] Although the content of the present invention has been described in detail through the above preferred embodiments, it should be appreciated that the above description should not be considered as a limitation of the present invention. After reading the above content, it will be apparent to those skilled in the art that various modifications and substitutions of the present invention will occur. Therefore, the protection scope of the present invention should be limited by the appended claims.

Claims

1. A method for preparing a porous graphene microsphere-based ultra-black coating, characterized in that: The following steps are included: (1) preparing graphene into a dispersion, dissolving 1-pyrene ester cyclodextrin in a sodium hydroxide aqueous solution and adding the resulting solution to the dispersion, ultrasonically obtaining a microsphere precursor solution, spraying the microsphere precursor solution into an organic solvent in an ethyl acetate ice bath, filtering the collected microspheres and freeze-drying them to obtain graphene / Py-CD microspheres having a porous structure; (2) preparing a resin solution, dispersing the obtained porous graphene / Py-CD microspheres in the resin solution to obtain a spraying precursor solution; (3) Spraying the spraying precursor liquid onto the surface of the material, and obtaining a porous graphene microsphere-based ultra-black coating after drying.

2. The preparation method according to claim 1, characterized in that: In the step (1), the dispersion is obtained by dispersing graphene in deionized water; the concentration of the sodium hydroxide aqueous solution is 0.1M; the spraying is performed using an air spray gun, the nozzle diameter of which is 0.3mm-0.8mm, and the working pressure is 1.5-4bar; the organic solvent is an organic solvent having a melting point lower than that of ethyl acetate and being immiscible with water, preferably selected from n-hexane, ether or 2-methylpentane; and the freeze-drying temperature is -80 degrees Celsius.

3. The preparation method according to claim 1, characterized in that: In the microsphere precursor solution in step (1), the final concentration of graphene is 2-6 mg / mL, the final concentration of 1-pyrene ester cyclodextrin is 0.1-2 mg / mL, and the particle size of the obtained graphene / Py-CD microspheres is 1-100 μm.

4. The preparation method according to claim 1, characterized in that: The resin solution in step (2) may be selected from any one of polydimethylsiloxane, polychlorotrifluoroethylene-vinylidene fluoride copolymer, polychlorotrifluoroethylene, polyvinylidene chloride, and polymethyl methacrylate, and the solvent for dissolving the resin may be selected from any one of acetone, ethanol, ethylene dichloride, n-hexane, tetrahydrofuran, cyclohexane, and dichloromethane.

5. The preparation method according to claim 1, characterized in that: The concentration of the resin in the resin solution of step (2) is 1wt% to 10wt%; the mass ratio of the resin to the porous graphene / Py-CD microspheres in the spraying precursor solution is 1:1 to 20:

1.

6. The preparation method according to claim 1, characterized in that: The spraying in step (3) is performed using an air spray gun, the nozzle diameter of which is 0.3 mm to 0.8 mm and the working pressure is 1.5 to 4 bar.

7. The preparation method according to claim 1, characterized in that: The material can be selected from aluminum plate, glass, paper, rubber or plastic.

8. The preparation method according to claim 1, characterized in that: The thickness of the obtained coating is 50 μm to 300 μm.

9. An ultra-black coating prepared by the preparation method according to any one of claims 1 to 8.

10. Use of the ultra-black coating as claimed in claim 9 in the field of anti-icing and in the preparation of materials with light absorption properties.

Citation Information

Patent Citations

  • Graphene aerogel microspheres and preparation method and application thereof

    CN105195067A

  • Preparation method of porous graphene microsphere ultra-black material

    CN112225202A

  • Carbon-based ultra-black stray light-eliminating nano-composite coating and preparation method thereof

    CN114479659A

  • Circuit board comprising ultra-black composite coating, display device and preparation method

    WO2023216715A1