Modified epoxy resin and preparation method thereof

By adding low-molecular monoepoxy compounds and polyurea polymers to epoxy resin, the cracking problem of epoxy resin coating in marine environment is solved, the impact resistance and self-repair ability are improved, and the service life is extended And reduces repair costs.

CN118931320AActive Publication Date: 2024-11-12JIMEI UNIV
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411001874.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-12
Estimated Expiration
2044-07-25

AI Technical Summary

Technical Problem

The existing epoxy resin coatings are susceptible to external impacts in marine environments, causing microcracks, resulting in pitting corrosion of the steel surface, short service life, and repair work mainly relies on labor, which is time-consuming and labor-intensive.

Method used

By adding low-molecular monoepoxy compounds and polyurea polymers to epoxy resins, the cross-linking density and toughness are reduced, the impact resistance of the coating is enhanced, and the self-healing performance is promoted through hydrogen bonds in polyurea polymers. .

Benefits of technology

It significantly improves the impact resistance and service life of the coating, and realizes self-healing function, reducing the dependence on manual repair.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118931320A_ABST
    Figure CN118931320A_ABST
Patent Text Reader

Abstract

The invention provides a modified epoxy resin and a preparation method thereof. The raw materials of the modified epoxy resin comprise epoxy resin and curing agent amine compounds, low-molecular single epoxy compounds and polyurea polymers. The preparation method of the modified epoxy resin comprises the following steps: reacting a bifunctional amine compound with a bifunctional isocyanate compound in an organic solvent to prepare a polyurea polymer; adding a low-molecular single epoxy compound into epoxy resin and stirring, then adding a curing agent amine compound and the polyurea polymer and stirring, removing bubbles in a system under vacuum negative pressure, and coating the surface of a substrate with the mixture to obtain the modified epoxy resin coating.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to the field of coatings, specifically to the field of material modification, and more specifically to modified epoxy resin and a preparation method thereof. Background Art

[0002] The chemical, electrochemical reactions and physical dissolution of metal materials in the marine environment will greatly shorten the life of marine engineering equipment. At present, in order to solve the corrosion problem of marine engineering equipment, researchers have proposed many targeted solutions, among which anti-corrosion coating is the most effective and most commonly used protection strategy.

[0003] Epoxy-based anti-corrosion coatings are favored by researchers for their high adhesion, low shrinkage and excellent resistance to chemical solvents. However, due to the rich benzene ring structure of epoxy resin, while it brings high adhesion to epoxy resin, it also makes it too rigid; in actual applications, it is very easy to produce microcracks when impacted by external forces, causing pitting on the surface of steel, greatly reducing the service life of the anti-corrosion coating and seriously endangering the safe operation of marine engineering equipment.

[0004] At present, most of the repair work of coating material damage is done manually, which is time-consuming and labor-intensive. Therefore, it has become a top priority for researchers to develop an anti-corrosion coating with long service life, excellent anti-corrosion performance and self-repairing function. Summary of the invention

[0005] In order to solve the problems existing in the background technology, the present disclosure provides a modified epoxy resin and a preparation method thereof. The raw materials of the modified epoxy resin include epoxy resin and a curing agent amine compound, and also include a low molecular weight monoepoxy compound and a polyurea polymer.

[0006] In some embodiments, the low molecular weight monoepoxy compound includes at least one of n-butyl glycidyl ether, allyl glycidyl ether, phenyl glycidyl ether, and 5-ethylhexyl glycidyl ether.

[0007] In some embodiments, the polyurea polymer includes a compound prepared by reacting a difunctional amine compound with a difunctional isocyanate compound in an organic solvent.

[0008] In some embodiments, the difunctional amine compound includes at least one of polyamide, polyetheramine, isophoronediamine, and diethylenetriamine.

[0009] In some embodiments, the difunctional isocyanate compound includes at least one of isophorone diisocyanate, toluene diisocyanate, diphenylmethane diisocyanate, and hexamethylene diisocyanate.

[0010] The preparation method of the modified epoxy resin comprises the following steps: S1: reacting a difunctional amine compound with a difunctional isocyanate compound in an organic solvent to obtain a polyurea polymer; S2: adding a low molecular weight monoepoxy compound to the epoxy resin and stirring, then adding a curing agent amine compound and the polyurea polymer and stirring, applying the mixture on the surface of a substrate after removing bubbles in the system by vacuum negative pressure to obtain a modified epoxy resin coating.

[0011] In some embodiments, the reaction temperature of step S1 is 10-120° C., and the reaction time is 2-24 hours.

[0012] In some embodiments, in step S1, the molar ratio of the difunctional amine compound to the difunctional isocyanate compound is (1-10):(0.1-10).

[0013] In some embodiments, in step S2, the mass ratio of the epoxy resin, the low molecular weight monoepoxy compound, the polyurea polymer and the curing agent amine compound is (0.1-30): (0.1-30): (0.01-10): (0.01-10).

[0014] In some embodiments, step S1 is: dissolving a difunctional amine compound in an organic solvent to form an organic solution, introducing nitrogen to remove air in the device, and then placing the device in an ice water bath; adding a difunctional isocyanate compound dropwise to the organic solution at a constant pressure to react and obtain a polyurea polymer.

[0015] The beneficial effects of the present disclosure are as follows: the epoxy resin composite material provided by the present disclosure can increase the impact resistance of the coating and provide the coating with a self-repairing function, thereby greatly extending the service life of the anti-corrosion coating. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 IR spectra of the epoxy coatings in Examples 1-7.

[0017] Figure 2 Graph showing the adhesion of each epoxy coating in Examples 1-7.

[0018] Figure 3 Graph showing the impact resistance of each epoxy coating in Examples 1-7.

[0019] Figure 4 Graph showing the open circuit potential of each epoxy coating in Examples 1-7.

[0020] Figure 5 The impedance diagram at 0.01 Hz of each epoxy coating in Examples 1-7. DETAILED DESCRIPTION

[0021] It should be understood that the disclosed embodiments are only examples of the present disclosure, and the present disclosure can be implemented in various forms. Therefore, the specific details of the present disclosure should not be interpreted as limitations, but only as the basis for the claims to teach those of ordinary skill in the art to implement the present disclosure in various ways. In the description of the present disclosure, the terms and professional terms that are not clearly described are common knowledge of those skilled in the art, and the methods that are not clearly described are conventional methods known to those skilled in the art.

[0022] The endpoints of the ranges and any values ​​disclosed in the present disclosure are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, and these numerical ranges should be deemed to be specifically disclosed herein.

[0023] [Modified epoxy resin]

[0024] The modified epoxy resin provided by the present invention reduces the crosslinking density of the epoxy coating by adding a low molecular weight monoepoxy compound to achieve self-healing performance; and then adds a polyurea polymer to increase the soft segment to improve the toughness of the epoxy coating; and the polyurea polymer is rich in hydrogen bonds, and its supramolecular force also helps to improve the self-healing performance of the epoxy coating.

[0025] The modified epoxy resin provided by the present disclosure comprises epoxy resin and a curing agent amine compound, and is characterized in that it also comprises a low molecular weight monoepoxy compound and a polyurea polymer.

[0026] In some embodiments, the epoxy resin includes at least one of E51, E44, E20, and E12. In some embodiments, the curing agent amine compound includes at least one of polyamide, polyetheramine, isophorone diamine, and diethylenetriamine.

[0027] In some embodiments, the low molecular weight monoepoxy compound includes at least one of n-butyl glycidyl ether, allyl glycidyl ether, phenyl glycidyl ether, and 5-ethylhexyl glycidyl ether.

[0028] In some embodiments, the mass ratio of the epoxy resin to the low molecular weight monoepoxy compound is (1-20): (0.1-10).

[0029] In some embodiments, the polyurea polymer includes a compound prepared by reacting a difunctional amine compound with a difunctional isocyanate compound in an organic solvent. In some embodiments, the difunctional amine compound includes at least one of polyamide, polyetheramine, isophorone diamine, and diethylene triamine. In some embodiments, the difunctional isocyanate compound includes at least one of isophorone diisocyanate, toluene diisocyanate, diphenylmethane diisocyanate, and hexamethylene diisocyanate. In some embodiments, the molar ratio of the difunctional amine compound to the difunctional isocyanate compound is (1 to 10): (0.1 to 10). In some embodiments, the mass ratio of the epoxy resin, the low molecular weight monoepoxy compound, the polyurea polymer, and the curing agent amine compound is (0.1 to 30): (0.1 to 30): (0.01 to 10): (0.01 to 10).

[0030] In some embodiments, the organic solvent includes at least one of dichloromethane, chloroform, N,N-dimethylformamide, acetone, and tetrahydrofuran.

[0031] [Preparation method of modified epoxy resin]

[0032] The preparation method of the modified epoxy resin provided by the present invention comprises the following steps: S1: reacting a difunctional amine compound with a difunctional isocyanate compound in an organic solvent to obtain a polyurea polymer; S2: adding a low molecular weight monoepoxy compound to the epoxy resin and stirring, then adding a curing agent amine compound and the polyurea polymer and stirring, applying the mixture on the surface of a substrate after removing bubbles in the system by vacuum negative pressure to obtain a modified epoxy resin coating.

[0033] <For S1>

[0034] In some embodiments, the difunctional amine compound includes at least one of polyamide, polyetheramine, isophorone diamine, and diethylene triamine. In some embodiments, the difunctional isocyanate compound includes at least one of isophorone diisocyanate, toluene diisocyanate, diphenylmethane diisocyanate, and hexamethylene diisocyanate. In some embodiments, the molar ratio of the difunctional amine compound to the difunctional isocyanate compound is (1-10): (0.1-10).

[0035] In some embodiments, the organic solvent includes at least one of dichloromethane, chloroform, N,N-dimethylformamide, acetone, and tetrahydrofuran.

[0036] In some embodiments, the reaction temperature in S1 is 10-120° C., and the reaction time is 2-24 h.

[0037] In some embodiments, the step S1 is: dissolving a difunctional amine compound in an organic solvent to form an organic solution, introducing nitrogen to remove air in the device, and then placing it in an ice-water bath; adding a difunctional isocyanate compound to the organic solution at a constant pressure to react and obtain a polyurea polymer. In some embodiments, the constant pressure addition is carried out using a constant pressure titration funnel. In some embodiments, the nitrogen introduction time is 15 min to 30 min. In some embodiments, the reaction time is 15 h to 25 h.

[0038] <For S2>

[0039] In some embodiments, the epoxy resin includes at least one of E51, E44, E20, and E12.

[0040] In some embodiments, the curing agent amine compound includes at least one of polyamide, polyetheramine, isophorone diamine, and diethylene triamine.

[0041] In some embodiments, the low molecular weight monoepoxy compound includes at least one of n-butyl glycidyl ether, allyl glycidyl ether, phenyl glycidyl ether, and 5-ethylhexyl glycidyl ether.

[0042] In some embodiments, the mass ratio of the epoxy resin to the low molecular weight monoepoxy compound is (1-20): (0.1-10).

[0043] In some embodiments, the mass ratio of the epoxy resin, the low molecular weight monoepoxy compound, the polyurea polymer and the curing agent amine compound is (0.1-30): (0.1-30): (0.01-10): (0.01-10).

[0044] In some embodiments, the substrate comprises at least one of a metal substrate, a glass substrate, a ceramic substrate, an enamel substrate, a polymer substrate, and a composite substrate formed by the above substrates. In some embodiments, the metal substrate comprises carbon steel.

[0045] [Example]

[0046] The present disclosure is further described below in conjunction with the examples. In the following examples and comparative examples, the reagents, materials and instruments used, unless otherwise specified, can be obtained commercially or prepared by methods known in the art.

[0047] Example 1

[0048] Weigh 10g of epoxy E51 into a 100mL beaker, add 10g of n-butyl glycidyl ether; stir for 5min; add 5g of polyetheramine and stir for 5min; apply vacuum negative pressure for 1h to remove bubbles, and spin coat on the surface of Q235 carbon steel to obtain a self-healing epoxy coating 1.

[0049] Example 2

[0050] Weigh 25g of epoxy E20 into a 50mL beaker, add 10g of n-butyl glycidyl ether; stir for 5min; add 5g of polyetheramine and stir for 5min; apply vacuum negative pressure for 1h to remove bubbles, and spin coat on the surface of Q235 carbon steel to obtain a self-healing epoxy coating 2.

[0051] Example 3

[0052] Weigh 40g of epoxy E12 into a 50mL beaker, add 10g of n-butyl glycidyl ether; stir for 5min; add 5g of polyetheramine and stir for 5min; apply vacuum negative pressure for 1h to remove bubbles, and spin coat on the surface of Q235 carbon steel to obtain a self-healing epoxy coating 3.

[0053] Example 4

[0054] Step 1: Weigh 80g of polyetheramine and dissolve it in 60mL of anhydrous chloroform solution in a 250mL three-necked flask, place 4.44g of isophorone diisocyanate in a constant pressure titration funnel, keep the airtightness of the reaction device, and pass nitrogen for 20min to remove the air in the device; place the entire device in an ice water bath for reaction for 18h; prepare a polyurea polymer PI.

[0055] Step 2: Weigh 25g of epoxy E20 into a 50mL beaker, add 10g of n-butyl glycidyl ether; stir for 5min; add 5g of polyetheramine and 5g of polyurea polymer PI, stir for 5min; apply vacuum negative pressure for 1h to remove bubbles, and spin coat on the surface of Q235 carbon steel to obtain a self-healing toughened epoxy coating 1.

[0056] Example 5

[0057] Step 1: Weigh 80g of polyetheramine and dissolve it in 60mL of anhydrous chloroform solution in a 250mL three-necked flask, place 4.44g of isophorone diisocyanate in a constant pressure titration funnel, keep the airtightness of the reaction device, and pass nitrogen for 20min to remove the air in the device; place the entire device in an ice water bath for reaction for 18h; prepare a polyurea polymer PI.

[0058] Step 2: Weigh 25g of epoxy E20 into a 50mL beaker, add 10g of n-butyl glycidyl ether; stir for 5min; add 5g of polyetheramine and 10g of polyurea polymer PI, stir for 5min; apply vacuum negative pressure for 1h to remove bubbles, and spin coat on the surface of Q235 carbon steel to obtain a self-healing toughened epoxy coating 2.

[0059] Example 6

[0060] Step 1: Weigh 80g of polyetheramine and dissolve it in 60mL of anhydrous chloroform solution in a 250mL three-necked flask, place 4.44g of isophorone diisocyanate in a constant pressure titration funnel, keep the airtightness of the reaction device, and pass nitrogen for 20min to remove the air in the device; place the entire device in an ice water bath for reaction for 18h; prepare a polyurea polymer PI.

[0061] Step 2: Weigh 25g of epoxy E20 into a 50mL beaker, add 10g of n-butyl glycidyl ether; stir for 5min; add 5g of polyetheramine and 15g of polyurea polymer PI, stir for 5min; apply vacuum negative pressure for 1h to remove bubbles, and spin coat on the surface of Q235 carbon steel to obtain a self-healing toughened epoxy coating 3.

[0062] Example 7

[0063] Step 1: Weigh 80g of polyetheramine and dissolve it in 60mL of anhydrous chloroform solution in a 250mL three-necked flask, place 4.44g of isophorone diisocyanate in a constant pressure titration funnel, keep the airtightness of the reaction device, and pass nitrogen for 20min to remove the air in the device; place the entire device in an ice water bath for reaction for 18h; prepare a polyurea polymer PI.

[0064] Step 2: Weigh 25g of epoxy E20 into a 50mL beaker, add 10g of n-butyl glycidyl ether; stir for 5min; add 5g of polyetheramine and 20g of polyurea polymer PI, stir for 5min; apply vacuum negative pressure for 1h to remove bubbles, and spin coat on the surface of Q235 carbon steel to obtain a self-healing toughened epoxy coating 4.

[0065] The material parameters involved in Examples 1-7 are shown in Table 1. For ease of explanation, symbols are used in Table 1 to represent specific materials:

[0066] A: E51

[0067] B: E20

[0068] C:E12

[0069] D: n-butyl glycidyl ether

[0070] E: Polyetheramine

[0071] F: Polyurea polymer PI

[0072] The self-repairing epoxy coatings 1-3 and the self-repairing toughened epoxy coatings 1-4 in Examples 1-7 were respectively tested for infrared, adhesion, impact resistance, open circuit potential and electrochemical impedance spectroscopy. The test results are as follows: Figure 1 -5.

[0073] Table 1 Material parameters in Examples 1-7

[0074] Example No. A / g B / g C / g D / g E / g F / g Example 1 10 - - 10 5 - Example 2 - 25 - 10 5 - Example 3 - - 40 10 5 - Example 4 - 25 - 10 5 5 Example 5 - 25 - 10 5 10 Example 6 - 25 - 10 5 15 Example 7 - 25 - 10 5 20

[0075] Note: “-” means not included.

[0076] exist Figure 1 Among them, seven groups of modified samples were at 1100cm -1 The characteristic absorption peaks appeared at 1600cm -1 、1580cm -1 、1500cm -1 and 1460cm -1 The difference in the intensity of the characteristic absorption peaks at 3200-3450cm is caused by the stretching vibration of the benzene ring in the epoxy resin. -1 A broad and strong characteristic absorption peak was observed at 1236 cm-1, which corresponds to the stretching vibration peak caused by the -OH bond formed after the curing agent attacks the oxygen ring of the epoxy resin through amino nucleophilic attack during the epoxy curing reaction, which can prove the success of the ring-opening addition polymerization reaction. -1 The characteristic peaks of CN bonds can be observed, which also proves that the target product was successfully prepared.

[0077] exist Figure 2 In the left figure, the adhesion of Example 1 is relatively weak, 6.19±0.46MPa; the adhesion of Example 2 reaches 9.32±0.69MPa; and the adhesion of Example 3 is the lowest, only 5.98±0.45MPa. For the right figure, after adding polyurea, as the content of polyurea increases, the adhesion of the modified epoxy resin gradually increases, and the adhesion of Examples 4, 5, 6, and 7 are 10.53±0.51MPa, 10.72±0.41MPa, 10.82±0.68MPa, and 11.15±0.25MPa, respectively.

[0078] exist Figure 3 In the left figure, as the number of benzene ring structures in the epoxy resin increases, its rigidity increases, which in turn leads to a downward trend in impact resistance. Example 1 has the highest impact strength, reaching 90Kg·cm, while the impact strength of Example 2 drops to 70Kg·cm, and the impact strength of Example 3 is the lowest, only 20Kg·cm. Figure 3 In the right figure, as the polyurea content increases, the impact resistance of the epoxy resin is gradually improved. The impact strengths of Examples 4, 5, 6, and 7 are 90 Kg·cm, 100 Kg·cm, 100 Kg·cm, and 100 Kg·cm, respectively.

[0079] exist Figure 4 , Figure 5 The open circuit potential and low frequency impedance (|Z|) of seven modified epoxy resin samples immersed in 3.5wt.% NaCl solution were 0.01Hz ). The intact coating has a high open circuit potential and low-frequency impedance; the open circuit potential and low-frequency impedance drop sharply after being scratched; by observing whether the open circuit potential and low-frequency impedance are restored after the repair treatment, it can be judged whether it has self-healing properties. The modified epoxy resin of Examples 1-3 achieves a self-healing effect by reducing the cross-linking density and improving the mobility of the chain segments; but the mechanical properties are weak. Examples 4-7 improve the mechanical strength of the self-healing epoxy resin through polyurea. The addition of polyurea will react with the epoxy group, increase the cross-linking density, and reduce the self-healing performance; however, the hydrogen bonds between polyureas promote the self-healing performance. Therefore, the self-healing performance of Examples 5-6 is relatively low, but when the amount of polyurea added reaches a certain level, the self-healing effect will be improved. Figure 4 , Figure 5 The results show that among the above embodiments, embodiments 2, 3, 4, and 7 have good self-repairing properties.

[0080] In summary, the modified epoxy resin coating provided by the present invention reduces the crosslinking density of the coating and achieves self-healing performance by adding low-molecular monoepoxy compounds; the addition of polyurea polymer increases the soft segment and improves the toughness of the epoxy coating; and the polyurea polymer is rich in hydrogen bonds, and its supramolecular force helps to improve the self-healing performance of the epoxy coating.

[0081] The above description is only an example of the present disclosure and does not constitute any form of limitation to the present disclosure. Although the present disclosure is disclosed as above in the form of a preferred embodiment, it is not intended to limit the present disclosure. Any technician familiar with the profession, without departing from the scope of the technical solution of the present disclosure, using the technical content disclosed above to make slight changes or modifications are equivalent to equivalent implementation cases and are within the scope of the technical solution of the present disclosure.

Claims

1. A modified epoxy resin, the raw materials of which include epoxy resin and a curing agent amine compound, characterized in that: It also includes low molecular weight monoepoxy compounds and polyurea polymers.

2. The modified epoxy resin according to claim 1, characterized in that The low molecular weight monoepoxy compound includes at least one of n-butyl glycidyl ether, allyl glycidyl ether, phenyl glycidyl ether, and 5-ethylhexyl glycidyl ether.

3. The modified epoxy resin according to claim 1, characterized in that The polyurea polymer includes a compound prepared by reacting a difunctional amine compound with a difunctional isocyanate compound in an organic solvent.

4. The modified epoxy resin according to claim 3, characterized in that The bifunctional amine compound includes at least one of polyamide, polyetheramine, isophoronediamine and diethylenetriamine.

5. The modified epoxy resin according to claim 3, characterized in that The bifunctional isocyanate compound includes at least one of isophorone diisocyanate, toluene diisocyanate, diphenylmethane diisocyanate and hexamethylene diisocyanate.

6. A method for preparing a modified epoxy resin, characterized in that: Includes steps: S1: reacting a difunctional amine compound with a difunctional isocyanate compound in an organic solvent to prepare a polyurea polymer; S2: adding a low molecular weight monoepoxy compound to the epoxy resin and stirring, then adding a curing agent amine compound and the polyurea polymer and stirring, removing bubbles in the system by vacuum negative pressure, and coating the surface of the substrate to obtain a modified epoxy resin coating.

7. The method for preparing the modified epoxy resin according to claim 6, characterized in that: The reaction temperature of step S1 is 10-120° C., and the reaction time is 2-24 hours.

8. The method for preparing the modified epoxy resin according to claim 6, characterized in that: In step S1, the molar ratio of the difunctional amine compound to the difunctional isocyanate compound is (1-10):(0.1-10).

9. The method for preparing the modified epoxy resin according to claim 6, characterized in that: In step S2, the mass ratio of the epoxy resin, the low molecular weight monoepoxy compound, the polyurea polymer and the curing agent amine compound is (0.1-30): (0.1-30): (0.01-10): (0.01-10).

10. The method for preparing the modified epoxy resin according to claim 6, characterized in that: The step S1 is: dissolving a difunctional amine compound in an organic solvent to form an organic solution, introducing nitrogen to remove air in the device, and then placing the device in an ice water bath; and dripping a difunctional isocyanate compound into the organic solution at a constant pressure to react and obtain a polyurea polymer.

Citation Information

Patent Citations

  • Self-repair function dual-microcapsule composition and application on self-repair function protective coating layer

    CN108102456A

  • Polyurea paint composition having excellent Anti-corrosiveness, chemical-resistance and workability, and construction method using thereof

    KR101197197B1

  • Anti-abrasion coating for concrete surface of dam and method for brushing the same

    WO2014075412A1