Preparation method of polyaniline / carbon tube conductive anti-corrosion super-hydrophobic coating

The preparation of a superhydrophobic, conductive, and anti-corrosion coating using polyaniline/carbon nanotube composite materials solves the problem that traditional coatings cannot simultaneously possess both conductivity and corrosion resistance. This results in high conductivity and excellent corrosion resistance, while also enhancing the coating's mechanical strength and wear resistance.

CN118931369APending Publication Date: 2024-11-12INNER MONGOLIA UHV BRANCH OF STATE GRID INNER MONGOLIA EASTERN ELECTRIC POWER CO LTD +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411256959.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-09
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Traditional anti-corrosion coatings, while providing corrosion protection, cannot meet the conductivity requirements of certain applications, especially in fields such as electromagnetic shielding, electrostatic discharge, and electrochemical sensing.

Method used

By using polyaniline/carbon nanotube composite materials, a superhydrophobic and conductive anti-corrosion coating of polyaniline/carbon nanotubes is prepared to form a continuous conductive network. Combined with the redox properties of polyaniline, it provides cathodic protection, blocks corrosive media, and enhances the mechanical strength and toughness of the coating.

Benefits of technology

It significantly improves the conductivity and corrosion resistance of the coating, extends the service life of the substrate, enhances the mechanical strength and wear resistance of the coating, and exhibits excellent durability and corrosion resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118931369A_ABST
    Figure CN118931369A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a polyaniline / carbon tube conductive anti-corrosion super-hydrophobic coating. Firstly, a polyaniline solution is prepared; uniformly pouring the polyaniline solution on the substrate; and finally, spraying the modified carbon tube particle solution containing perfluorooctanoic acid on the surface of the prepared polyaniline matrix, and drying and curing to form the polyaniline / carbon tube super-hydrophobic conductive anticorrosive coating. The perfluorooctanoic acid is utilized to modify the carbon tube particles, and meanwhile, a polyaniline material is introduced, so that the coating has relatively good conductive and corrosion-resistant effects; the coating achieves the conductive and anti-corrosion characteristics through the micro-nano composite structure particles, and has the effect of limiting the surface aging of the coating.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of super hydrophobicity, and in particular relates to a method for preparing a polyaniline / carbon tube conductive anticorrosive super hydrophobic coating. Background Art

[0002] Conductive anti-corrosion coatings are a type of functional coating that has both electrical conductivity and anti-corrosion properties. They are widely used in marine engineering, chemical equipment, oil and gas pipelines, power equipment and other fields. The development of this type of coating aims to resolve the performance contradiction between traditional anti-corrosion coatings and conductive coatings, that is, while providing anti-corrosion protection, it is also necessary to maintain or give the material a certain degree of conductivity. Traditional anti-corrosion coatings usually prevent the contact between corrosive media and substrates through methods such as physical barriers, chemical inertness or sacrificial anodes. However, these coating materials often have insulating properties and cannot meet the needs of certain specific applications. For example, in the fields of electromagnetic shielding, electrostatic discharge, and electrochemical sensing, the coating is required to not only be anti-corrosive, but also have good conductivity.

[0003] The development of conductive anti-corrosion coatings involves the combination and innovation of multiple materials, including conductive polymers (such as polyaniline, polypyrrole), metal nanoparticles (such as silver, copper, nickel), carbon-based nanomaterials (such as graphene, carbon nanotubes), etc. These materials can be added to the coating by chemical, physical or composite methods to form an anti-corrosion coating with a conductive network structure. Conductive polymers have become one of the hot research materials in recent years due to their excellent chemical stability and conductivity. In addition, the application of nanotechnology also provides a new way to improve the conductivity and corrosion resistance of coatings. Summary of the invention

[0004] The purpose of the present invention is to disclose a method for preparing a polyaniline / carbon tube super-hydrophobic conductive anti-corrosion coating.

[0005] A method for preparing a conductive anti-corrosion super-hydrophobic composite coating is specifically achieved by the following steps:

[0006] S1, prepare substrate materials, clean and smooth the surface of the substrate, and record the treated surface as A for standby use;

[0007] S2, adding carbon tube particles into anhydrous ethanol, stirring magnetically at 800-1200 rpm at room temperature for 12-24 hours, and recording as solution B for later use;

[0008] S3, adding ammonia water and anhydrous ethanol to solution B, mixing by ultrasonic for 10-30 min, then adding tetraethyl orthosilicate and anhydrous ethanol dropwise at a rate of 1 ml / min to obtain a mixed solution C; stirring with a magnetic stirrer at a speed of 800-1200 rpm for 12-24 h at room temperature;

[0009] S4, adding perfluorooctyltriethoxysilane (POTS) to solution C to modify the surface of the solution, the reaction time is 1-8 hours, the solution is placed in an oven at 70-90° C. to dry, and dispersed with anhydrous ethanol to obtain solution D;

[0010] S5, adding epoxy resin and polyamide to solution D, mixing and stirring at a speed of 100-200 r / min for 10-20 min, obtaining a lower layer of viscous material after centrifugal separation, and dispersing it with butyl glycidyl ether to obtain a physically mixed solution E;

[0011] S6. Add sodium dodecylbenzene sulfonate, aniline and perfluorooctanoic acid (PFOA) into a flask; continuously stir and ultrasonicate in an ice-water bath; when the temperature drops below 5°C, slowly dropwise add sodium polydisulfide propane sulfonate (SPS), stir in an ice-water bath for 12-24 hours, and record as solution F;

[0012] S7. Pour solution F evenly onto substrate A after mixing, dry at 80-100° C. for 6-8 h, then spray solution E, and dry at 80-100° C. for 6-8 h to obtain a polyaniline / carbon tube super-hydrophobic conductive anti-corrosion coating.

[0013] Furthermore, in step S1, the substrate material can be aluminum alloy, copper alloy and steel, and its thickness is not less than 5 mm; the surface smoothing and cleaning treatment includes: using a belt grinding or grinding method to smooth the substrate surface until the roughness Ra value is less than 0.64 μm, and then using anhydrous ethanol and deionized water for ultrasonic cleaning respectively, each cleaning time is 20-30 minutes, and then drying for use.

[0014] Furthermore, in step S2, the specification of the carbon tube is 10-40 um, and the addition amount is (10-20) wt%.

[0015] Furthermore, in step S3, the volume ratio of ammonia water to anhydrous ethanol is (1-3): (60-120); the volume ratio of tetraethyl orthosilicate to anhydrous ethanol is (2-3): (20-25).

[0016] Furthermore, in step S4, the volume ratio of perfluorooctyltriethoxysilane to solution C is (1-2): (50-80).

[0017] Furthermore, in step S5, the mass ratio of solution D, epoxy resin and polyamide is (4-8):(1-3):(1-3).

[0018] Furthermore, in step S6, the molar ratio of sodium dodecylbenzene sulfonate, aniline and perfluorooctanoic acid (PFOA) is (2-6): (1000-2000): (1000-2000).

[0019] The concentration of sodium disulfide propane sulfonate in the sodium disulfide propane sulfonate (SPS) aqueous solution in step S6 is 0.05-0.15 mol, and the amount added dropwise is 5-10 wt%.

[0020] The beneficial effects of the present invention are as follows:

[0021] (1) Carbon nanotubes have extremely high electrical conductivity and can significantly improve the overall conductivity of the coating by forming a continuous conductive network in the coating. Polyaniline, as a conductive polymer, also contributes to some of the conductivity.

[0022] (2) Polyaniline has unique redox properties and can provide cathodic protection through doping / dedoping mechanisms to reduce corrosion of the substrate. Carbon nanotubes and polyaniline together form a dense coating structure that effectively blocks the corrosion of the substrate by oxygen, moisture and other corrosive media, thereby extending the service life of the substrate.

[0023] (3) The addition of carbon nanotubes significantly improves the mechanical strength and toughness of the coating, making the coating more resistant to wear and mechanical impact. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is a scanning electron microscope image of the surface microstructure of the coating prepared in Example 1.

[0025] Figure 2 , Figure 3 This is the equivalent circuit used to fit the EIS data in Example 2. DETAILED DESCRIPTION

[0026] In order to facilitate the understanding of the present invention, the present invention will be described more fully below. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.

[0027] Example 1

[0028] A method for preparing a polyaniline / carbon tube conductive anticorrosive super-hydrophobic composite coating is specifically carried out according to the following steps:

[0029] S1. Select 45# steel sheet and polish the surface by grinding process until the roughness Ra value is less than 0.64μm. Then, ultrasonically clean it in anhydrous ethanol and deionized water in turn, each time for 20min. The surface treated in this way is recorded as A and is naturally dried for later use.

[0030] S2, add 0.2 g of carbon tube particles into 20 mL of anhydrous ethanol, stir magnetically at 1000 rpm for 12 h at room temperature, and record it as solution B for later use;

[0031] S3, add 3 mL of ammonia water and 65 mL of anhydrous ethanol to solution B, mix ultrasonically for 20 min, then add 3 mL of tetraethyl orthosilicate and 25 mL of anhydrous ethanol dropwise at a rate of 1 mL / min to obtain a mixed solution C; stir with a magnetic stirrer at 800 rpm for 12 h at room temperature;

[0032] S4, adding 3 mL of perfluorooctyltriethoxysilane (POTS) to solution C to modify the surface of the solution, the reaction time is 8 h, the solution is placed in an oven at 80° C. to dry, and dispersed in 10 mL of anhydrous ethanol to obtain solution D;

[0033] S5. Add epoxy resin and polyamide to solution D, mix and stir at a speed of 150 r / min for 15 min, and after centrifugation, the mass ratio of solution D, epoxy resin and polyamide is 6:1:1, and the lower layer of viscous material is obtained and dispersed with 10 mL of butyl glycidyl ether to obtain a physically mixed solution E;

[0034] S6. Add 0.04mmol sodium dodecylbenzenesulfonate, 0.01mol aniline and 0.01mol PFOA into a flask; continuously stir and ultrasonicate in an ice-water bath; when the temperature drops below 5°C, slowly dropwise add an aqueous solution containing 0.1mol SPS in an amount of 8wt%; stir in an ice-water bath for 12h, and record it as solution F;

[0035] S7. Pour 50 mg of solution F evenly onto substrate A after mixing, dry at 80° C. for 6 h, then spray solution E, and dry at 80° C. for 6 h to obtain a polyaniline / carbon tube super-hydrophobic conductive anti-corrosion coating.

[0036] Example 2

[0037] A method for preparing a polyaniline / carbon tube conductive anticorrosive super-hydrophobic composite coating is specifically carried out according to the following steps:

[0038] S1. Select a 6061 aluminum alloy sheet, and use a grinding process to perform surface finishing processing on the sheet until the roughness Ra value is less than 0.64 μm. Then, ultrasonically clean the sheet in anhydrous ethanol and deionized water in turn, each time for 20 minutes. The surface treated in this way is recorded as A, and is naturally dried for later use;

[0039] S2, add 0.25g carbon tube particles into 20mL anhydrous ethanol, stir magnetically at 900rpm for 12h at room temperature, and record it as solution B for later use;

[0040] S3, add 3 mL of ammonia water and 65 mL of anhydrous ethanol to solution B, mix ultrasonically for 20 min, then add 3 mL of tetraethyl orthosilicate and 25 mL of anhydrous ethanol dropwise at a rate of 1 mL / min to obtain a mixed solution C; stir with a magnetic stirrer at 800 rpm for 12 h at room temperature;

[0041] S4, adding 3 mL of perfluorooctyltriethoxysilane (POTS) to solution C to modify the surface of the solution, the reaction time is 8 h, the solution is placed in an oven at 80° C. to dry, and dispersed in 10 mL of anhydrous ethanol to obtain solution D;

[0042] S5. Add epoxy resin and polyamide to solution D, mix and stir at a speed of 150 r / min for 15 min, and after centrifugation, the mass ratio of solution D, epoxy resin and polyamide is 6:2:1, and the lower layer of viscous material is obtained and dispersed with 10 mL of butyl glycidyl ether to obtain a physically mixed solution E;

[0043] S6. Add 0.03mmol sodium dodecylbenzenesulfonate, 0.01mol aniline and 0.01mol PFOA to the flask; stir continuously and ultrasonicate in an ice-water bath. When the temperature drops below 5°C, slowly drop 0.1mol SPS aqueous solution in an amount of 6wt%; stir in an ice-water bath for 12h, and record it as solution F.

[0044] S7. Pour 50 mg of solution F evenly onto substrate A after mixing, dry at 80° C. for 6 h, then spray solution E, and dry at 80° C. for 6 h to obtain a polyaniline / carbon tube super-hydrophobic conductive anti-corrosion coating.

[0045] Example 3

[0046] A method for preparing a polyaniline / carbon tube conductive anticorrosive super-hydrophobic composite coating is specifically carried out according to the following steps:

[0047] S1. Select alumina ceramics and polish the surface by grinding until the roughness Ra value is less than 0.64 μm. Then, ultrasonically clean the surface in anhydrous ethanol and deionized water in turn, each time for 20 minutes. The surface treated in this way is recorded as A and dried naturally for later use.

[0048] S2, add 0.25g carbon tube particles into 20mL anhydrous ethanol, stir magnetically at 1200rpm for 12h at room temperature, and record it as solution B for later use;

[0049] S3, add 3 mL of ammonia water and 65 mL of anhydrous ethanol to solution B, mix ultrasonically for 20 min, then add 3 mL of tetraethyl orthosilicate and 25 mL of anhydrous ethanol dropwise at a rate of 1 mL / min to obtain a mixed solution C; stir with a magnetic stirrer at 800 rpm for 12 h at room temperature;

[0050] S4, adding 3 mL of perfluorooctyltriethoxysilane (POTS) to solution C to modify the surface of the solution, the reaction time is 8 h, the solution is placed in an oven at 80° C. to dry, and dispersed in 10 mL of anhydrous ethanol to obtain solution D;

[0051] S5. Add epoxy resin and polyamide to solution D, mix and stir at a speed of 150 r / min for 15 min, and after centrifugation, the mass ratio of solution D, epoxy resin and polyamide is 6:1:2, and the lower layer of viscous material is obtained and dispersed with 10 mL of butyl glycidyl ether to obtain a physically mixed solution E;

[0052] S6. Add 0.03 mmol sodium dodecylbenzene sulfonate, 0.01 mol aniline and 0.01 mol PFOA into a flask; continuously stir and ultrasonicate in an ice-water bath; when the temperature drops below 5°C, slowly dropwise add 0.1 mol SPS aqueous solution in an amount of 9 wt %; stir in an ice-water bath for 12 h, recorded as solution F;

[0053] S7. Pour 50 mg of solution F evenly onto substrate A after mixing, dry at 80° C. for 6 h, then spray solution E, and dry at 80° C. for 6 h to obtain a polyaniline / carbon tube super-hydrophobic conductive anti-corrosion coating.

[0054] Experimental Example 1

[0055] The erosion medium consisted of pure water and SiC particles with a diameter of about 150 μm, with a SiC concentration of 15%. The erosion time was 20 minutes, and the impact rate was maintained at 3.13 m·s -1 , the impact angle is 90°. After reaching the time, the coating is cleaned and weighed to analyze its corrosion resistance. Figure 1 The microscopic morphology formed on the coating surface was examined by scanning electron microscopy. Under the high-speed impact of SiC particles, the mass loss and volume loss of the coating were 451.33 mg and 240.50 mm, respectively. 3 When 1wt%, 2.5wt% and 3.5wt% of polyaniline filler were introduced into the coating, the mass loss was reduced by 12.37%, 22.83% and 23.24%, respectively, and the corresponding volume loss was reduced by 14.01%, 32.73% and 43.85%, respectively, compared with the coating without polyaniline, indicating that the corrosion resistance of the prepared coating is enhanced with the increase of polyaniline filler concentration.

[0056] In this section, the wear resistance of the polyaniline / carbon tube conductive anti-corrosion coating described in the present invention is analyzed. On the one hand, it provides reference and support for technical research in related fields, and on the other hand, the data show that the super hydrophobic coating provided by the present invention has excellent wear resistance and durability.

[0057] Experimental Example 2

[0058] Electrochemical impedance spectroscopy (EIS) tests were performed on the coatings under a 10 mV sinusoidal perturbation and a measurement frequency range of 100 kHz to 0.01 Hz. The electrolyte for EIS measurements was 3.5 wt% NaCl solution. The corrosion time was set to 1 day and 7 days.

[0059] Table 1 shows the relevant resistance values ​​of the coatings when the corrosion time is set to 1 day and 7 days. The charge transfer resistance (R CT ) is 2.01×10 7 Ω·cm 2 After immersion in 3.5wt% NaCl solution for 7 days, the coating exhibited excellent corrosion resistance with a resistance of 1.56×10 8 Ω·cm 2 When the corrosive medium comes into contact with the metal substrate, corrosion products are formed on its surface and begin to diffuse. However, the polyaniline / carbon tube coating makes the substrate passivated and the corrosion inhibition performance significantly reduces or even eliminates the diffusion rate of corrosion products. Figure 2 and Figure 3 is the equivalent circuit used to fit the EIS data.

[0060] The electrochemical impedance spectroscopy (EIS) test of the coatings with different polyaniline and perfluorooctanoic acid mass ratios was then investigated, and the electrolyte was 3.5wt% NaCl solution. The results showed that when the ratio of polyaniline to perfluorooctanoic acid was 1.0:1.5, the polyaniline / carbon nanotube composite coating exhibited the most effective conductive anticorrosion performance.

[0061] Table 1 Equivalent circuit fitting of electrochemical parameters measured by EIS

[0062] sample <![CDATA[R s (Ωcm 2 )]]> <![CDATA[R f (Ωcm 2 )]]> <![CDATA[R CT (Ωcm 2 )]]> A(1 day) <![CDATA[1.65×10 7 ]]> <![CDATA[1.32×10 7 ]]> <![CDATA[2.01×10 7 <!-- 4 -->]]> B(7 days) <![CDATA[5.51×10 8 ]]> <![CDATA[8.01×10 8 ]]> <![CDATA[1.56×10 8 ]]>

[0063] In this section, the corrosion resistance of the polyaniline / carbon tube conductive anti-corrosion coating described in the present invention is analyzed. On the one hand, it provides reference and support for technical research in related fields, and on the other hand, the data shows that the super hydrophobic coating provided by the present invention has good conductivity and durability.

[0064] Example 3

[0065] Referring to the surface contact angle / rolling angle standard measurement test, the conductive / anticorrosive super-hydrophobic composite coatings of Examples 1-3 were tested for contact angle and rolling angle, and the medium was distilled water. The test results are shown in Table 2.

[0066] Table 2 Contact angle and rolling angle test results of conductive / anticorrosive super-hydrophobic composite coatings of Examples 1-3

[0067] Contact angle (°) Roll angle (°) Example 1 165.6 2.6 Example 2 154.4 7.4 Example 3 141.4 7.0

[0068] The above results show that the surface energy of different substrate materials has an effect on the contact angle of the polyaniline / carbon tube hydrophobic coating. High surface energy substrates tend to show smaller contact angles. This is because high surface energy materials can enhance the interaction between the coating and the substrate, thereby changing the microstructure and surface energy state of the coating. Conversely, low surface energy substrates are more likely to form large contact angles.

[0069] The above embodiments 1-3 are described in detail for better understanding and use of the present invention. It is particularly pointed out here that for ordinary technicians in the field, without departing from the design spirit of the present invention, making several variations and modifications to the present invention should fall within the protection scope of the present invention. The protection scope of the patent of the present invention shall be based on the attached claims.

Claims

1. A method for preparing a polyaniline / carbon tube conductive anticorrosive super-hydrophobic coating, It is characterized in that The following steps are involved: S1, prepare substrate materials, clean and smooth the surface of the substrate, and record the treated surface as A for standby use; S2, adding carbon tube particles into anhydrous ethanol, stirring magnetically at 800-1200 rpm at room temperature for 12-24 hours, and recording as solution B for later use; S3, adding ammonia water and anhydrous ethanol to solution B, mixing by ultrasonic for 10-30 min, then adding tetraethyl orthosilicate and anhydrous ethanol dropwise at a rate of 1 mL / min to obtain a mixed solution C, and stirring with a magnetic stirrer at a speed of 800-1200 rpm for 12-24 h at room temperature; S4, adding perfluorooctyl triethoxysilane to solution C to modify the surface of the solution, the reaction time is 1-8 hours, the solution is placed in an oven at 70-90°C for drying, and dispersed with anhydrous ethanol to obtain solution D; S5, adding epoxy resin and polyamide to solution D, mixing and stirring at a speed of 100-200 r / min for 10-20 min, obtaining a lower layer of viscous material after centrifugal separation, and dispersing it with butyl glycidyl ether to obtain a physically mixed solution E; S6. Add sodium dodecylbenzene sulfonate, aniline and perfluorooctanoic acid into a flask; continuously stir and ultrasonicate in an ice-water bath; when the temperature drops below 5°C, slowly dropwise add a sodium polydisulfide dipropane sulfonate aqueous solution, stir in an ice-water bath for 12-24 hours, and record it as solution F; S7. Pour solution F evenly onto substrate A after mixing, dry at 80-100° C. for 6-8 h, then spray solution E, and dry at the same temperature for 6-8 h to obtain a polyaniline / carbon tube super-hydrophobic conductive anti-corrosion coating.

2. The method for preparing the polyaniline / carbon tube conductive anticorrosive super hydrophobic coating according to claim 1, It is characterized in that The step S1 includes: S1.1 The substrate material is aluminum alloy, copper alloy or steel, and its thickness is not less than 5mm; S1.2 Surface leveling and cleaning: Use belt grinding or grinding to level the substrate surface until the roughness Ra value is less than 0.64μm, then use anhydrous ethanol and deionized water for ultrasonic cleaning respectively, each cleaning time is 20-30min, and then set aside after drying.

3. The method for preparing the polyaniline / carbon tube conductive anticorrosive super hydrophobic coating according to claim 1, It is characterized in that In step S2, the carbon tube particles have a specification of 10-40 um and a content of (10-20) wt%.

4. The method for preparing the polyaniline / carbon tube conductive anticorrosive super hydrophobic coating according to claim 1, It is characterized in that In step S3, the volume ratio of ammonia water to anhydrous ethanol is (1-3): (60-120); the volume ratio of tetraethyl orthosilicate to anhydrous ethanol is (2-3): (20-25).

5. The method for preparing the polyaniline / carbon tube conductive anticorrosive super hydrophobic coating according to claim 1, It is characterized in that In step S4, the volume ratio of perfluorooctyltriethoxysilane to solution C is (1-2): (50-80).

6. The method for preparing the polyaniline / carbon tube conductive anticorrosive super hydrophobic coating according to claim 1, It is characterized in that In the step S5, the mass ratio of solution D, epoxy resin and polyamide is (4-8):(1-3):(1-3).

7. The method for preparing the polyaniline / carbon tube conductive anticorrosive super-hydrophobic coating according to claim 1, It is characterized in that In step S6, the molar ratio of sodium dodecylbenzenesulfonate, aniline and perfluorooctanoic acid is (2-6): (1-2): (1-2).

8. The method for preparing the polyaniline / carbon tube conductive anticorrosive super hydrophobic coating according to claim 1, It is characterized in that The concentration of sodium disulfide bis(propylene disulfide) in the sodium disulfide bis(propylene disulfide) aqueous solution in step S6 is 0.05-0.15 mol, and the amount added dropwise is 5-10 wt%.

Citation Information

Cited By

  • Ultraviolet-absorption corrosion-resistant super-hydrophobic PMMA (polymethyl methacrylate) coating and preparation method thereof

    CN121108834A