Graphene antibacterial film and preparation method thereof
By modifying the graphene powder and spraying it on the surface of the substrate, the antibacterial rate and bonding strength of the graphene antibacterial film are improved, and the problem of limited antibacterial effect caused by graphene powder dispersion in the prior art is solved, thus achieving the goal of achieving the problem of the dispersion of graphene powder in the prior art. It has efficient antibacterial effect and long-life graphene antibacterial film.
Patent Information
- Application Number
- CN202411169598.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-24
- Publication Date
- 2024-11-12
AI Technical Summary
In the existing graphene antibacterial film, graphene powder is dispersed inside the antibacterial layer, and the antibacterial effect is limited, so it is necessary to improve the antibacterial effect and antibacterial rate.
Using modified graphene powder, tetrahydrophthalic anhydride, N,N-bis(3-aminopropyl)ethylethylamine, 3-(methacryloyloxy)propyltrimethoxysilane, trimethoxysilane Hydroxymethylpropane triacrylate and allyl trimethylammonium chloride were treated to form graphene powder with modified groups, and sprayed on the surface of the substrate to improve antibacterial effect and bonding strength.
The antibacterial rate of graphene antibacterial membrane was significantly improved, with the antibacterial rate of Staphylococcus aureus >99%, the antibacterial rate of Escherichia coli >96%, and the antibacterial rate of Candida albicans >89%, and the adhesive and The bonding strength of the substrate extends the service life.
Smart Images

Figure BDA0005008844560000081
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of functional materials, and more specifically, to a graphene antibacterial film and a preparation method thereof. Background Art
[0002] With the improvement of people's living standards, antibacterial materials have been widely used in many fields such as medical treatment, food packaging, biological experiments and public health. Graphene powder can act on bacterial cells by producing inactive oxygen free radicals, thereby achieving a sterilizing effect. It can also inhibit the formation of biofilms, inhibit the survival and spread of bacteria, and its sharp edges can also puncture the cell walls of bacteria, causing the cell contents to leak, thereby eliminating bacteria. It can also interfere with the metabolic process of bacteria, inhibit bacterial growth and reproduction, and it can also enhance the permeability of cell membranes, leading to the loss of intracellular substances and inhibiting bacterial activity. Also because graphene powder has good antibacterial properties, it has been used in the application of antibacterial films. Graphene antibacterial films in the prior art generally include a substrate, an antibacterial layer is arranged on the surface of the substrate, and the antibacterial layer is often mixed with an adhesive and graphene to obtain a mixture, and then the mixture is coated on the surface of the substrate, and after curing, an antibacterial layer is formed. However, graphene powder is dispersed inside the antibacterial layer, and the antibacterial effect is limited, which needs to be further improved. Summary of the invention
[0003] In order to improve the antibacterial effect, the present application provides a graphene antibacterial film and a preparation method thereof.
[0004] In a first aspect, the present application provides a graphene antibacterial film, which adopts the following technical solution: A graphene antibacterial film comprises a substrate and an adhesive layer arranged on the surface of the substrate; the surface of the adhesive layer is provided with the antibacterial layer; the raw material of the adhesive layer is an adhesive; the antibacterial layer is formed by spraying modified graphene powder on the surface of the adhesive and curing the adhesive; the modified graphene powder is obtained by treating graphene powder with tetrahydrophthalic anhydride, N,N-di(3-aminopropyl)ethylethylamine, 3-(methacryloyloxy)propyltrimethoxysilane, trimethylolpropane triacrylate and allyltrimethylammonium chloride.
[0005] By adopting the above technical scheme, an antibacterial layer is set on the surface of the substrate, and the antibacterial property of the antibacterial layer is utilized to make the graphene antibacterial film have certain antibacterial properties. At the same time, modified graphene powder is sprayed on the surface of the substrate, and the modified graphene powder is tightly adhered to the surface of the substrate through an adhesive, thereby increasing the amount of surface modified graphene powder and improving the antibacterial effect. In addition, the graphene powder is modified, which not only further improves the antibacterial rate, but also increases the bonding strength between it and the adhesive and the substrate, so that the modified graphene powder has the advantages of good adhesion and strong bonding, thereby increasing the stability and life of the graphene antibacterial film. The antibacterial rate of the graphene antibacterial film against Staphylococcus aureus is greater than 99%, the antibacterial rate against Escherichia coli is greater than 96%, the antibacterial rate against Candida albicans is greater than 89%, and the abrasion amount is less than 0.1 mg / m 2 , which makes the graphene antibacterial film have the characteristics of good antibacterial effect and strong bonding of modified graphene powder, and has excellent market application prospects.
[0006] Optionally, the modified graphene powder is prepared by the following method: T1. Mix toluene and tetrahydrophthalic anhydride, add N,N-di(3-aminopropyl)ethylethylamine, stir for 1-3h, concentrate under reduced pressure, dry to obtain an intermediate with a double bond, and set aside; T2, adding graphene powder to water, ultrasonically treating for 20-40 min, adding 3-(methacryloyloxy)propyltrimethoxysilane, stirring for 1-3 h, filtering, and obtaining silane-grafted graphene; T3, adding silane-grafted graphene to water, mixing, adding the double bond intermediate obtained in step T1, trimethylolpropane triacrylate, and allyltrimethylammonium chloride, mixing, adding a cross-linking agent, stirring for 2-4 hours, filtering, washing, and drying to obtain modified graphene powder.
[0007] Optionally, the weight ratio of the graphene powder, 3-(methacryloyloxy)propyltrimethoxysilane, double bond intermediate, trimethylolpropane triacrylate, and allyltrimethylammonium chloride is 100:(9-11):(4-6):(4-6):(4-6).
[0008] By adopting the above technical scheme, the anhydride group in tetrahydrophthalic anhydride and the secondary amine group in N,N-di(3-aminopropyl)ethylethylamine are first reacted to form a double-bonded intermediate, which contains not only a carbon-carbon double bond but also an amino group and a carboxyl group.
[0009] 3-(Methacryloyloxy)propyltrimethoxysilane is grafted on the surface of graphene powder to introduce a carbon-carbon double bond, and then a double-bonded intermediate, trimethylolpropane triacrylate, and allyltrimethylammonium chloride are added, and a cross-linking agent is used to cause a polymerization reaction to achieve grafting, introduce amine groups, carboxyl groups, ester groups, and quaternary ammonium salt groups, and increase the number of groups on the surface of the graphene powder. Since trimethylolpropane triacrylate contains three carbon-carbon double bonds and three side chains, the number of side chains is also increased, thereby enhancing the bonding strength between the modified graphene powder and the adhesive, improving the adhesion of the modified graphene powder, and extending the service life.
[0010] Optionally, the weight ratio of the graphene powder to the cross-linking agent is 100:(0.2-0.3).
[0011] By adopting the above technical solution, the amount of cross-linking agent added is optimized, which facilitates the control of the amount of cross-linking agent added.
[0012] Optionally, the cross-linking agent is one or more of ammonium persulfate, sodium persulfate, and potassium persulfate. In multiple embodiments, the cross-linking agent is ammonium persulfate, and the cross-linking agent can also be set to sodium persulfate or potassium persulfate as needed, but is not limited to the listed options, and other options not listed within the selection range are also applicable.
[0013] Optionally, the weight ratio of tetrahydrophthalic anhydride and N,N-di(3-aminopropyl)ethylethylamine is (7-11):(4-6).
[0014] By adopting the technical scheme, the weight ratio of tetrahydrophthalic anhydride and N,N-di(3-aminopropyl)ethylethylamine is optimized, so as to facilitate the reaction of tetrahydrophthalic anhydride and N,N-di(3-aminopropyl)ethylethylamine.
[0015] Optionally, in step T1, the weight ratio of tetrahydrophthalic anhydride and toluene is (7-11):(80-120).
[0016] Optionally, in step T2, the weight ratio of the graphene powder to water is 1:(7-13).
[0017] Optionally, in step T3, the weight ratio of trimethylolpropane triacrylate and water is (4-6):(700-1300).
[0018] Optionally, the average particle size of the graphene powder is 50-100 nm.
[0019] By adopting the above technical solution, the particle size of the graphene powder is limited, which not only increases the stability of the raw material source, but also ensures the antibacterial effect of the graphene powder. In multiple embodiments, the average particle size of the graphene powder is 70nm, and the average particle size can also be set to 50nm, 60nm, 80nm, 90nm, 100nm as needed, but it is not limited to the listed values, and other values not listed in the numerical range are also applicable.
[0020] Optionally, the substrate is one of PET film, LDPE film, HDPE film, PVC film, and PP film. In multiple embodiments, the substrate is a PET film, and the substrate can also be set to LDPE film, HDPE film, PVC film, and PP film as needed, but it is not limited to the listed options, and other options not listed within the selection range are also applicable.
[0021] Optionally, the thickness of the substrate is 10-500 μm. Preferably, the thickness of the substrate is 10-300 μm. More preferably, the thickness of the substrate is 10-100 μm. In multiple embodiments, the thickness of the substrate is 50 μm, and the thickness of the substrate can also be set to 10 μm, 12 μm, 25 μm, 75 μm, 100 μm, 125 μm, 150 μm, 200 μm, 250 μm, 300 μm as needed, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0022] Optionally, the adhesive is one or more of polyurethane glue, polyamide glue, acrylate glue, and epoxy resin glue.
[0023] By adopting the above technical solution, the adhesive is optimized, which facilitates the selection of the adhesive.
[0024] Optionally, the substrate is pretreated as follows before use: Add tris(hydroxymethyl)aminomethane) into water and mix, adjust the pH value to 8-9, add dopamine hydrochloride and mix, immerse the substrate, stir and treat for 10-15 hours, take out the substrate, dry it, and obtain the pretreated substrate.
[0025] Optionally, the weight ratio of the substrate, water, tris(hydroxymethyl)aminomethane, and dopamine hydrochloride is 100:(700-1300):(5-7):(7-9).
[0026] By adopting the above technical scheme, before the substrate is used, the substrate is soaked with dopamine hydrochloride and dopamine is grafted on the surface of the substrate, which greatly increases the number of active groups on the surface of the substrate, enhances the bonding strength between the substrate and the adhesive layer, improves the peel strength of the adhesive layer, and also improves the adhesion of the modified graphene powder, thereby extending the stability and life of the graphene antibacterial film.
[0027] In a second aspect, the present application provides a method for preparing the graphene antibacterial film, which adopts the following technical solution: A method for preparing the graphene antibacterial film comprises the following steps: S1. Apply the adhesive on the surface of the substrate. The coating amount of the adhesive is 0.3-0.5g / m 2 , and forming an adhesive layer; S2. Spraying modified graphene powder on the surface of the adhesive layer, the spraying amount of modified graphene powder is 0.6-1 mg / m 2 Then, a release paper is attached to the surface, and the temperature is raised to 60-80°C under a pressure of 0.6-0.8MPa, and the curing treatment is performed for 50-70min. The release paper is torn off, the adhesive layer forms an adhesive layer, and the modified graphene powder forms an antibacterial layer to obtain a graphene antibacterial film.
[0028] Compared with adding modified graphene powder to an adhesive to obtain a mixture, and then coating the mixture on the surface of a substrate, the preparation method of the present application first coats the adhesive on the surface of the substrate, and then sprays the modified graphene powder on the surface of the adhesive. At this time, most of the modified graphene powder is embedded in the adhesive surface, and the remaining modified graphene powder is embedded in the adhesive, thereby increasing the amount of modified graphene powder on the surface of the graphene antibacterial film and improving the antibacterial effect.
[0029] In summary, this application has at least the following beneficial effects: 1. The graphene antibacterial film of the present application is modified by graphene powder, which not only further improves the antibacterial rate, making the antibacterial rate of Staphylococcus aureus greater than 99%, the antibacterial rate of Escherichia coli greater than 96%, and the antibacterial rate of Candida albicans greater than 89%, but also increases the bonding strength between it and the adhesive and the substrate, and the wear amount is less than 0.1mg / m 2 That is, the graphene antibacterial film of the present application not only has the characteristics of good antibacterial effect, but the modified graphene powder also has the advantages of good adhesion and strong bonding, which prolongs the antibacterial time and service life, and has excellent market application prospects.
[0030] 2. The preparation method of the graphene antibacterial film of the present application is to first apply an adhesive on the surface of the substrate, and then spray the modified graphene powder on the surface of the adhesive. At this time, most of the modified graphene powder is embedded in the adhesive surface, and the remaining modified graphene powder is embedded in the adhesive, thereby increasing the amount of surface modified graphene powder and improving the antibacterial effect. DETAILED DESCRIPTION
[0031] In order to make the present application easier to understand, the present application will be further described in detail below in conjunction with the examples, which are merely illustrative and are not intended to limit the scope of application of the present application. The raw materials or components used in the present application can be obtained through commercial routes or conventional methods unless otherwise specified.
[0032] Preparation Example Preparation Example 1 A modified graphene powder is prepared by the following method: T1. Add 9 g of tetrahydrophthalic anhydride to 100 g of toluene at a speed of 800 r / min and stir for 3 min. Then add 5 g of N,N-di(3-aminopropyl)ethylethylamine and stir for 2 h. Then, concentrate under reduced pressure to remove most of the toluene, and then dry to remove the remaining toluene to obtain a double bond intermediate for standby use.
[0033] T2. Add 100 g of graphene powder to 1000 g of water and perform ultrasonic treatment for 30 min. Then, add 10 g of 3-(methacryloyloxy)propyltrimethoxysilane at a speed of 400 r / min and stir for 2 h. Then, filter to obtain silane-grafted graphene.
[0034] Among them, the average particle size of the graphene powder is 70nm, and it is selected from Nangong Jiuxin New Material Technology Co., Ltd.
[0035] T3, at a speed of 400r / min, add all the silane-grafted graphene obtained in step T2 to 1000g of water, and stir for 3min. Then add 5g of the double-bonded intermediate obtained in step T1, 5g of trimethylolpropane triacrylate, and 5g of allyltrimethylammonium chloride, and stir for 3min. Then add 0.25g of a cross-linking agent and stir for 3h. Then filter and wash with water three times, with 500g of water added each time. Then dry to obtain modified graphene powder.
[0036] Wherein, the cross-linking agent is ammonium persulfate.
[0037] Preparation Example 2 A modified graphene powder is prepared by the following method: T1. Add 11 g of tetrahydrophthalic anhydride to 100 g of toluene at a speed of 800 r / min and stir for 3 min. Then add 4 g of N,N-di(3-aminopropyl)ethylethylamine and stir for 1 h. Then, concentrate under reduced pressure to remove most of the toluene, and then dry to remove the remaining toluene to obtain an intermediate with a double bond for standby use.
[0038] T2. Add 100 g of graphene powder to 1000 g of water and perform ultrasonic treatment for 20 min. Then, add 9 g of 3-(methacryloyloxy)propyltrimethoxysilane at a speed of 400 r / min and stir for 1 h. Then, filter to obtain silane-grafted graphene.
[0039] Among them, the average particle size of the graphene powder is 70nm, and it is selected from Nangong Jiuxin New Material Technology Co., Ltd.
[0040] T3, at a speed of 400r / min, add all the silane-grafted graphene obtained in step T2 to 1000g of water, and stir for 3min. Then add 6g of the double-bonded intermediate obtained in step T1, 4g of trimethylolpropane triacrylate, and 6g of allyltrimethylammonium chloride, and stir for 3min. Then add 0.2g of a cross-linking agent and stir for 2h. Then filter and wash with water three times, with 500g of water added each time. Then dry to obtain modified graphene powder.
[0041] Wherein, the cross-linking agent is ammonium persulfate.
[0042] Preparation Example 3 A modified graphene powder is prepared by the following method: T1. Add 7 g of tetrahydrophthalic anhydride to 100 g of toluene at a rotation speed of 800 r / min and stir for 3 min. Then add 6 g of N,N-di(3-aminopropyl)ethylethylamine and stir for 3 h. Then, concentrate under reduced pressure to remove most of the toluene, and then dry to remove the remaining toluene to obtain an intermediate with a double bond for standby use.
[0043] T2. Add 100 g of graphene powder to 1000 g of water and perform ultrasonic treatment for 40 min. Then, add 11 g of 3-(methacryloyloxy)propyltrimethoxysilane at a speed of 400 r / min and stir for 3 h. Then, filter to obtain silane-grafted graphene.
[0044] Among them, the average particle size of the graphene powder is 70nm, and it is selected from Nangong Jiuxin New Material Technology Co., Ltd.
[0045] T3, at a speed of 400r / min, add all the silane-grafted graphene obtained in step T2 to 1000g of water, and stir for 3min. Then add 4g of the double-bonded intermediate obtained in step T1, 6g of trimethylolpropane triacrylate, and 4g of allyltrimethylammonium chloride, and stir for 3min. Then add 0.3g of a cross-linking agent and stir for 4h. Then filter and wash with water three times, with 500g of water added each time. Then dry to obtain modified graphene powder.
[0046] Wherein, the cross-linking agent is ammonium persulfate. Example
[0047] Example 1 A graphene antibacterial film, the graphene antibacterial film comprises a substrate, the substrate is a PET film, the thickness of the PET film is 50 μm. An adhesive layer is arranged on the surface of the substrate, the adhesive layer is processed by an adhesive, the adhesive is a polyurethane adhesive, and the polyurethane adhesive is Henkel DORUS MD 3287. An antibacterial layer is arranged on the surface of the adhesive layer, the antibacterial layer is formed by spraying modified graphene powder on the surface of the adhesive and curing the adhesive, and the modified graphene powder is prepared by the method of Preparation Example 1.
[0048] A method for preparing a graphene antibacterial film comprises the following steps: S1. Use a coating machine to apply the adhesive on the surface of the substrate. The coating amount of the adhesive is 0.4g / m 2 , and an adhesive layer is formed.
[0049] S2. Use electrostatic spraying to spray modified graphene powder on the surface of the adhesive layer. The spraying amount of modified graphene powder is 0.8 mg / m 2 Then, a release paper is attached to the surface, and the temperature is raised to 70°C under a pressure of 0.7 MPa, and the curing treatment is performed for 60 minutes. The release paper is torn off, the adhesive layer forms an adhesive layer, and the modified graphene powder forms an antibacterial layer to obtain a graphene antibacterial film.
[0050] S3. Roll up the graphene antibacterial film and put it into storage.
[0051] Example 2 A graphene antibacterial film, which is different from Example 1 in that the modified graphene powder used in the antibacterial layer has a different source, and the modified graphene powder is prepared by the method of Preparation Example 2.
[0052] Example 3 A graphene antibacterial film, which is different from Example 1 in that the modified graphene powder used in the antibacterial layer has a different source, and the modified graphene powder is prepared by the method of Preparation Example 3.
[0053] Example 4 A graphene antibacterial film, which is different from Example 1 in that the substrate is pretreated before use, and the pretreatment adopts the following method: At a speed of 200 r / min, 6 g of tris(hydroxymethyl)aminomethane was added to 1000 g of water and stirred for 5 min. Then, a 15% hydrochloric acid aqueous solution was used to adjust the pH value to 8.5. Then, 8 g of dopamine hydrochloride was added and stirred for 10 min. Then, 100 g of the substrate was immersed and stirred for 13 h. The substrate was taken out and dried to obtain the pretreated substrate.
[0054] Example 5 A graphene antibacterial film, which is different from Example 1 in that the substrate is pretreated before use, and the pretreatment adopts the following method: At a speed of 200 r / min, 5 g of tris(hydroxymethyl)aminomethane was added to 700 g of water and stirred for 5 min. Then, a 15% hydrochloric acid aqueous solution was used to adjust the pH value to 9. Then, 9 g of dopamine hydrochloride was added and stirred for 10 min. Then, 100 g of the substrate was immersed and stirred for 15 h. The substrate was taken out and dried to obtain the pretreated substrate.
[0055] Example 6 A graphene antibacterial film, which is different from Example 1 in that the substrate is pretreated before use, and the pretreatment adopts the following method: At a speed of 200 r / min, 7 g of tris(hydroxymethyl)aminomethane was added to 1300 g of water and stirred for 5 min. Then, a 15% hydrochloric acid aqueous solution was used to adjust the pH value to 8. Then, 7 g of dopamine hydrochloride was added and stirred for 10 min. Then, 100 g of the substrate was immersed and stirred for 10 h. The substrate was taken out and dried to obtain the pretreated substrate.
[0056] Comparative Example Comparative Example 1 A graphene antibacterial film, which differs from Example 1 in that an equal amount of graphene powder is used to replace modified graphene powder in the antibacterial layer.
[0057] Comparative Example 2 A graphene antibacterial film, which is different from Example 1 in that the silane-grafted graphite oxide powder used in the antibacterial layer replaces the modified graphene powder in equal amounts, and the silane-grafted graphite oxide powder is prepared by the following method: 100 g of graphene powder was added to 1000 g of water and ultrasonically treated for 30 min. Then, 10 g of 3-(methacryloyloxy)propyltrimethoxysilane was added at a speed of 400 r / min and stirred for 2 h. Afterwards, the mixture was filtered and washed three times with water, each time with 500 g of water added. Afterwards, the mixture was dried to obtain silane-grafted graphene powder.
[0058] Among them, the average particle size of the graphene powder is 70nm, and it is selected from Nangong Jiuxin New Material Technology Co., Ltd.
[0059] Comparative Example 3 A graphene antibacterial film, which differs from Example 1 in that in the preparation method of the modified graphene powder used in the antibacterial layer, in step T3, trimethylolpropane triacrylate is replaced by an equal amount of an intermediate with a double bond.
[0060] Comparative Example 4 A graphene antibacterial film, which differs from Example 1 in that in the preparation method of the modified graphene powder used in the antibacterial layer, in step T3, an equal amount of trimethylolpropane triacrylate is used to replace the double-bonded intermediate.
[0061] Comparative Example 5 A graphene antibacterial film, which differs from Example 1 in that in the preparation method of the modified graphene powder used in the antibacterial layer, in step T3, allyltrimethylammonium chloride is replaced with an equal amount of water.
[0062] Performance Testing The graphene antibacterial films obtained in Examples 1-6 and Comparative Examples 1-5 were taken as samples, and the following performance tests were performed on the samples. The test results are shown in Table 1.
[0063] Among them, the antibacterial rate of the graphene antibacterial film was tested in accordance with QB / T2591-2003 "Test methods and antibacterial effects of antibacterial plastics".
[0064] According to GB / T9867-2008 "Determination of wear resistance of vulcanized rubber or thermoplastic rubber (rotating roller abrader method)", the wear amount of the graphene antibacterial film was tested, and the smaller the wear amount, the better the adhesion of the modified graphene powder.
[0065] According to GB / T2791-1995 "Adhesive T peel strength test method - Flexible material to flexible material", the peel strength of the adhesive layer of the graphene antibacterial film was tested, and the greater the peel strength, the better the bonding strength of the adhesive layer.
[0066] Table 1 Test results As can be seen from Table 1, the graphene antibacterial film of the present application has a high antibacterial rate, with an antibacterial rate of 99.3-99.7% for Staphylococcus aureus, 96.3-96.6% for Escherichia coli, and 89.4-89.7% for Candida albicans, showing the advantage of high antibacterial rate. It also has a low wear amount, which is 0.05-0.09 mg / m 2 , showing the advantage of good adhesion of modified graphene powder, thereby extending the antibacterial time. At the same time, it also has a high peel strength of 6.13-6.86N / 2.5cm, showing the advantage of good bonding strength of the adhesive layer, thereby extending the service life. That is, the graphene antibacterial film of the present application has the characteristics of good antibacterial effect, strong bonding of graphene powder, and stable bonding of the adhesive layer, extending the stability and life of the graphene antibacterial film, and meeting market demand.
[0067] Comparative Example 1 and Comparative Example 2 are compared. Graphene powder is used in the antibacterial layer of Comparative Example 1, and silane-grafted graphite oxide powder is used in the antibacterial layer of Comparative Example 2. It can be seen that the modification of graphene powder with 3-(methacryloyloxy)propyltrimethoxysilane does not substantially affect the antibacterial rate, but significantly reduces the amount of wear, which is beneficial to improving the bonding stability. Combined with Comparative Examples 2-4 and Example 1, modified graphene powder is used in the antibacterial layer of Comparative Example 3, and 3-(methacryloyloxy)propyltrimethoxysilane, a double bond intermediate, and propyltrimethylammonium chloride are used to modify the graphene powder; modified graphene powder is used in the antibacterial layer of Comparative Example 4, and 3-(methacryloyloxy)propyltrimethoxysilane, trimethylolpropane triacrylate, and propyltrimethylammonium chloride are used to modify the graphene powder; modified graphene powder is used in the antibacterial layer of Example 1, and 3-(methacryloyloxy)propyltrimethoxysilane, a double bond intermediate, trimethylolpropane triacrylate, and propyltrimethylammonium chloride are used to modify the graphene powder. It can be seen from this that on the basis of using 3-(methacryloyloxy)propyltrimethoxysilane to treat the graphene powder, trimethylolpropane triacrylate, a double-bond intermediate, is further used for grafting, and the synergistic effect between the two is utilized to significantly improve the adhesion of the modified graphene powder, increase the stability of the modified graphene powder, and prolong the antibacterial time without affecting the antibacterial property.
[0068] Comparing Example 1 with Comparative Example 5, the modified graphene powder of Comparative Example 5 uses 3-(methacryloyloxy)propyltrimethoxysilane, a double-bonded intermediate, and trimethylolpropane triacrylate to modify the graphene powder; the modified graphene powder of Example 1 uses 3-(methacryloyloxy)propyltrimethoxysilane, a double-bonded intermediate, trimethylolpropane triacrylate, and propyltrimethylammonium chloride to modify the graphene powder. It can be seen that the antibacterial property of the graphene antibacterial film can be significantly improved by treating the graphene powder with propyltrimethylammonium chloride and grafting quaternary ammonium salt groups on the graphene surface.
[0069] By comparing Example 1 with Example 4, it can be seen that pretreatment of the substrate does not substantially affect the antibacterial properties of the graphene antibacterial film, but significantly increases the peel strength of the adhesive layer, increases the stability of the adhesive layer, and also increases the stability of the modified graphene powder, thereby extending the service life of the graphene antibacterial film.
[0070] It should be noted that the embodiments described above are only used to explain the present application and do not constitute any limitation to the present application. The present application is described with reference to typical embodiments, but it should be understood that the words used therein are descriptive and explanatory words, rather than restrictive words. The present application may be modified as specified within the scope of the claims of the present application, and the present invention may be revised without departing from the scope and spirit of the present application. Although the present application described therein relates to specific methods, materials and embodiments, it does not mean that the present application is limited to the specific examples disclosed therein. On the contrary, the present application can be extended to all other methods and applications with the same functions.
Claims
1. A graphene antibacterial film, characterized in that: The graphene antibacterial film includes a substrate and an adhesive layer arranged on the surface of the substrate. The antibacterial layer is arranged on the surface of the adhesive layer. The raw material of the adhesive layer is an adhesive. The antibacterial layer is formed by spraying modified graphene powder on the surface of the adhesive and curing the adhesive. The modified graphene powder is obtained by treating graphene powder with tetrahydrophthalic anhydride, N,N-bis(3-aminopropyl)ethylethylamine, 3-(methacryloyloxy)propyltrimethoxysilane, trimethylolpropane triacrylate, and allyltrimethylammonium chloride.
2. A graphene antibacterial film according to claim 1, characterized in that: The modified graphene powder is prepared by the following method: T1. Mix toluene and tetrahydrophthalic anhydride, add N,N-bis(3-aminopropyl)ethylethylamine, stir for 1-3 hours, concentrate under reduced pressure, and dry to obtain an intermediate with a double bond, which is set aside; T2. Add graphene powder to water, ultrasonicate for 20-40 min, add 3-(methacryloyloxy)propyltrimethoxysilane, stir for 1-3 h, and filter to obtain silane-grafted graphene; T3. Add silane-grafted graphene to water and mix, add the double bond intermediate obtained in step T1, trimethylolpropane triacrylate, and allyltrimethylammonium chloride and mix, add a cross-linking agent, stir for 2-4 hours, filter, wash, and dry to obtain modified graphene powder.
3. A graphene antibacterial film according to claim 2, characterized in that: The weight ratio of the graphene powder, 3-(methacryloyloxy)propyltrimethoxysilane, double bond intermediate, trimethylolpropane triacrylate and allyltrimethylammonium chloride is 100:(9-11):(4-6):(4-6):(4-6).
4. A graphene antibacterial film according to claim 2, characterized in that: The weight ratio of the graphene powder to the cross-linking agent is 100:(0.2-0.3).
5. A graphene antibacterial film according to claim 2, characterized in that: The weight ratio of the tetrahydrophthalic anhydride and N,N-bis(3-aminopropyl)ethylethylamine is (7-11):(4-6).
6. A graphene antibacterial film according to claim 2, characterized in that: The average particle size of the graphene powder is 50-100 nm.
7. The graphene antibacterial film according to claim 1, characterized in that: The adhesive is one or more of polyurethane glue, polyamide glue, acrylate glue and epoxy resin glue.
8. The graphene antibacterial film according to claim 1, characterized in that: The substrate was pretreated as follows before use: Tris(hydroxymethyl)aminomethane) is added to water and mixed, and the pH value is adjusted to 8-9. Dopamine hydrochloride is added and mixed, and the mixture is immersed in the substrate, and the substrate is stirred for 10-15 hours. The substrate is taken out and dried to obtain a pretreated substrate.
9. The graphene antibacterial film according to claim 8, characterized in that: The weight ratio of the substrate, water, tris(hydroxymethyl)aminomethane and dopamine hydrochloride is 100:(700-1300):(5-7):(7-9).
10. A method for preparing a graphene antibacterial film according to any one of claims 1 to 9, characterized in that: The steps include: S1. Apply adhesive on the surface of the substrate. The coating amount of adhesive is 0.3-0.5g / m 2 , and forming an adhesive layer; S2. Spray modified graphene powder on the surface of the adhesive layer. The spraying amount of modified graphene powder is 0.6-1 mg / m 2 Then, a release paper is attached to the surface, and the temperature is raised to 60-80°C under a pressure of 0.6-0.8MPa, and the curing treatment is performed for 50-70min. The release paper is torn off, the adhesive layer forms an adhesive layer, and the modified graphene powder forms an antibacterial layer to obtain a graphene antibacterial film.