High-viscosity / degradable acrylate pressure-sensitive adhesive and preparation method thereof
The high viscosity/degradable acrylate pressure-sensitive adhesive prepared through specific ratios and process steps solves the problem of insufficient degradability of acrylate pressure-sensitive adhesives in the prior art, and achieves the combination of high viscosity and degradability, improving the improvement of The durability and application fields of the product.
Patent Information
- Application Number
- CN202411107634.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-11-12
AI Technical Summary
Existing acrylate pressure-sensitive adhesives lack degradability and will reduce their base bonding properties when improving degradability.
It is made of propan-2-ene-1-ylcarbamate, 4-methyl-1,2-dithicyclopentane-4-carboxylic acid, 3-methoxyacrylic acid, isobutyl cinnamate, High viscosity/degradable acrylate pressure-sensitive adhesive composed of dodecano methacrylate, heat initiator and solvent are prepared through specific ratios and process steps, including heating, nitrogen protection, and mixed solution droplets of monomer initiator Add and keep warm and cool to form an adhesive with excellent bonding ability and degradability.
It realizes high viscosity and degradable acrylate pressure-sensitive adhesive, maintains viscosity performance for a long time, improves the durability and reliability of the product, and has good degradation capabilities.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of pressure-sensitive adhesives, and in particular to a high-viscosity / degradable acrylate pressure-sensitive adhesive and a preparation method thereof. Background Art
[0002] Acrylic pressure-sensitive adhesive is a self-adhesive material that can form a relatively strong bond under a small force. It is a type of adhesive that can be tightly bonded to the adherend with just a slight finger pressure without the need for solvents, heat or other means. This pressure-sensitive bonding performance is its most basic characteristic and a significant feature that distinguishes it from other types of adhesives.
[0003] Most of the acrylic pressure-sensitive adhesives currently produced and used in the market lack degradability. The main reason why acrylic pressure-sensitive adhesives are not degradable is the insolubility of the cross-linked network structure and the difficulty of breaking the CC of the main chain structure. Free radical ring-opening polymerization, as an important polymerization method, can synthesize polymer materials with specific structures and properties that can be degraded under specific conditions, but this method will reduce the basic performance of pressure-sensitive adhesives.
[0004] Therefore, there is an urgent need to propose a high-viscosity, degradable acrylate pressure-sensitive adhesive and a preparation method thereof to solve the above technical problems. Summary of the invention
[0005] The purpose of the present invention is to solve the problem that the degradable material formed by the common technology cannot take into account the performance. A brief summary of the present invention is given below to provide a basic understanding of certain aspects of the present invention. It should be understood that this summary is not an exhaustive summary of the present invention. It is not intended to determine the key or important parts of the present invention, nor is it intended to limit the scope of the present invention.
[0006] The technical solution of the present invention:
[0007] A high-viscosity / degradable acrylate pressure-sensitive adhesive, which is composed of prop-2-en-1-yl carbamate, 4-methyl-1,2-dithiolane-4-carboxylic acid, 3-methoxyacrylic acid, isobutyl cinnamate, behenyl methacrylate, a thermal initiator, and a solvent;
[0008] The mass fraction of prop-2-en-1-ylcarbamate is 20-40 parts, the mass fraction of 4-methyl-1,2-dithiolane-4-carboxylic acid is 30-80 parts, the mass fraction of 3-methoxyacrylic acid is 1-5 parts, the mass fraction of isobutyl cinnamate is 20-30 parts, the mass fraction of behenyl methacrylate is 30-60 parts, the mass fraction of thermal initiator is 0.3-0.8 parts, and the mass fraction of solvent is 190-300 parts.
[0009] Preferably, the thermal initiator is one or more of benzoyl peroxide, tert-butyl peroxyvalerate, azobisisobutyronitrile, or dodecanoyl peroxide.
[0010] Preferably, the solvent is one or more of toluene, butyl acetate, propyl acetate and ethyl propionate.
[0011] A method for preparing a high-viscosity / degradable acrylic pressure-sensitive adhesive comprises the following steps:
[0012] Step 1: Put part of the solvent into a reaction container, heat the reaction container, and introduce nitrogen protection after heating;
[0013] Step 2: Propylene-2-en-1-ylcarbamate, 4-methyl-1,2-dithiolane-4-carboxylic acid, 3-methoxyacrylic acid, isobutyl cinnamate, docosyl methacrylate, part of the thermal initiator and part of the solvent are mixed and stirred to obtain a monomer initiator mixed solution;
[0014] Step 3: Add the monomer-initiator mixed solution dropwise to the reaction container, and keep warm after the addition is completed;
[0015] Step 4: Mix the thermal initiator and the solution and stir them evenly to obtain an initiator mixed solution, and drop the initiator mixed solution into the reaction container;
[0016] Step 5: After the initiator mixed solution is added dropwise, the mixture is kept warm, stirred and cooled to room temperature to obtain a high viscosity / degradable acrylic pressure-sensitive adhesive.
[0017] Preferably, the stirring rate is 150-200 r / min, and the temperature of the reaction container in step 1 is raised to 75-95°C.
[0018] Preferably: the insulation time is 1.5h.
[0019] Preferably, in step 3, the monomer-initiator mixed solution is added dropwise to the reaction container through a constant pressure dropping funnel for 1-6 hours, and in step 4, the adding time is 15 minutes.
[0020] The present invention has the following beneficial effects:
[0021] The acrylic pressure-sensitive adhesive prepared by the present invention has excellent bonding ability and is degradable.
[0022] The acrylic pressure-sensitive adhesive prepared by the invention has stable performance, can maintain viscosity for a long time, is not easy to fall off or fail, and improves the durability and reliability of the product. DETAILED DESCRIPTION
[0023] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is described below by the specific embodiments shown. However, it should be understood that these descriptions are only exemplary and are not intended to limit the scope of the present invention. In addition, in the following description, the description of known structures and technologies is omitted to avoid unnecessary confusion of the concept of the present invention.
[0024] Specific implementation method 1: This implementation method is a high-viscosity / degradable acrylate pressure-sensitive adhesive, a high-viscosity / degradable acrylate pressure-sensitive adhesive, the high-viscosity / degradable acrylate pressure-sensitive adhesive is composed of prop-2-en-1-yl carbamate, 4-methyl-1,2-dithiolane-4-carboxylic acid, 3-methoxyacrylic acid, isobutyl cinnamate, behenyl methacrylate, a thermal initiator, and a solvent;
[0025] The mass fraction of prop-2-en-1-ylcarbamate is 20-40 parts, the mass fraction of 4-methyl-1,2-dithiolane-4-carboxylic acid is 30-80 parts, the mass fraction of 3-methoxyacrylic acid is 1-5 parts, the mass fraction of isobutyl cinnamate is 20-30 parts, the mass fraction of behenyl methacrylate is 30-60 parts, the mass fraction of thermal initiator is 0.3-0.8 parts, and the mass fraction of solvent is 190-300 parts.
[0026] Preferably, the mass fraction of prop-2-en-1-ylcarbamate is 30-35 parts, the mass fraction of 4-methyl-1,2-dithiolane-4-carboxylic acid is 40-60 parts, the mass fraction of 3-methoxyacrylic acid is 3 parts, the mass fraction of isobutyl cinnamate is 25 parts, the mass fraction of behenyl methacrylate is 40-50 parts, and the mass fraction of thermal initiator is 0.4-0.5 parts.
[0027] Specific implementation method 2: This implementation method is a high-viscosity / degradable acrylic pressure-sensitive adhesive, wherein the thermal initiator is one or more of benzoyl peroxide, tert-butyl peroxyvalerate, azobisisobutyronitrile, or dodecanoyl peroxide.
[0028] Specific implementation method three: In this implementation method, a high-viscosity / degradable acrylic pressure-sensitive adhesive is used, and the solvent is one or more of toluene, butyl acetate, propyl acetate, and ethyl propionate.
[0029] Specific embodiment 4: A method for preparing a high-viscosity / degradable acrylic pressure-sensitive adhesive in this embodiment comprises the following steps:
[0030] Step 1: Put part of the solvent into a reaction container, heat the reaction container, and introduce nitrogen protection after heating;
[0031] Step 2: Propylene-2-en-1-ylcarbamate, 4-methyl-1,2-dithiolane-4-carboxylic acid, 3-methoxyacrylic acid, isobutyl cinnamate, docosyl methacrylate, part of the thermal initiator and part of the solvent are mixed and stirred to obtain a monomer initiator mixed solution;
[0032] Step 3: Add the monomer-initiator mixed solution dropwise to the reaction container, and keep warm after the addition is completed;
[0033] Step 4: Mix the thermal initiator and the solution and stir them evenly to obtain an initiator mixed solution, and drop the initiator mixed solution into the reaction container;
[0034] Step 5: After the initiator mixed solution is added dropwise, the mixture is kept warm, stirred and cooled to room temperature to obtain a high viscosity / degradable acrylic pressure-sensitive adhesive.
[0035] Specific implementation method 5: In this implementation method, a method for preparing a high-viscosity / degradable acrylic pressure-sensitive adhesive is provided, wherein the stirring rate is 150-200 r / min, and in step 1, the temperature of the reaction container is raised to 75-95° C. to promote the polymerization reaction.
[0036] Specific implementation method six: In the preparation method of a high-viscosity / degradable acrylic pressure-sensitive adhesive of this implementation method, the heat preservation time is 1.5 hours to promote the polymerization reaction.
[0037] Specific implementation method seven: This implementation method is a method for preparing a high-viscosity / degradable acrylic pressure-sensitive adhesive. In step three, the monomer initiator mixed solution is added dropwise to the reaction container through a constant pressure dropping funnel for 1-6 hours. In step four, the adding time is 15 minutes to ensure that the reaction is carried out under mild conditions.
[0038] The present invention is described in detail below in conjunction with various embodiments, but it should be noted that these embodiments are not limitations of the present invention, and any equivalent transformations or substitutions in functions, methods, or structures made by ordinary technicians in the field based on these embodiments are all within the scope of protection of the present invention.
[0039] Example 1
[0040] This embodiment discloses a high-viscosity / degradable acrylate pressure-sensitive adhesive and a preparation method thereof, comprising the following steps:
[0041] Step 1: Place 90 g of toluene into a reaction vessel, heat to 80°C, and introduce nitrogen protection;
[0042] Step 2: Weigh 20 g of prop-2-en-1-ylcarbamate, 30 g of 4-methyl-1,2-dithiolane-4-carboxylic acid, 1 g of 3-methoxyacrylic acid, 20 g of isobutyl cinnamate, 60 g of behenyl methacrylate, 0.2 g of dibenzoyl peroxide and 90 g of toluene, mix and stir evenly to form a monomer initiator mixed solution, and stir at a speed of 200 r / min;
[0043] Step 3: Add the prepared monomer-initiator mixed solution to the reaction vessel through a constant pressure dropping funnel. The dropping time is 5 hours. After the dropping is completed, keep warm for 1.5 hours.
[0044] Step 4: 0.1 g of dibenzoyl peroxide and 10 g of toluene were mixed and stirred to form an initiator mixture, and the initiator mixture was added dropwise to the reaction container to initiate polymerization of the remaining monomers. The stirring speed was 200 r / min and the dropping time was 15 min.
[0045] Step 5: After the initiator mixed solution is added dropwise, keep the mixture warm for 1.5 hours, and stir and cool to room temperature to obtain a high-viscosity / degradable acrylic pressure-sensitive adhesive.
[0046] Example 2
[0047] This embodiment discloses a high-viscosity / degradable acrylate pressure-sensitive adhesive and a preparation method thereof, comprising the following steps:
[0048] Step 1: Place 120 g of ethyl propionate into a reaction vessel and heat to 80°C. Pass nitrogen gas for protection:
[0049] Step 2: 40 g of prop-2-en-1-ylcarbamate, 80 g of 4-methyl-1,2-dithiolane-4-carboxylic acid, 5 g of 3-methoxyacrylic acid, 30 g of isobutyl cinnamate, 30 g of behenyl methacrylate, 0.6 g of dodecyl peroxide and 170 g of ethyl propionate were mixed and stirred to form a monomer initiator mixture at a stirring speed of 200 r / min;
[0050] Step 3: Add the prepared monomer-initiator mixed solution to the reaction vessel through a constant pressure dropping funnel. The dropping time is 5 hours. After the dropping is completed, keep warm for 1.5 hours.
[0051] Step 4: 0.2 g of dodecyl peroxide and 10 g of ethyl propionate were mixed evenly to form an initiator mixture, and the initiator mixture was added dropwise to the reaction container to initiate polymerization of the remaining monomers. The stirring speed was 200 r / min and the dropping time was 15 min.
[0052] Step 5: After the initiator mixed solution is added dropwise, keep the mixture warm for 1.5 hours, and stir and cool to room temperature to obtain a high-viscosity / degradable acrylic pressure-sensitive adhesive.
[0053] Example 3
[0054] Step 1: Place 100 g of butyl acetate into a reaction vessel, heat to 75°C, and introduce nitrogen protection;
[0055] Step 2: 25 g of prop-2-en-1-ylcarbamate, 50 g of 4-methyl-1,2-dithiolane-4-carboxylic acid, 2 g of 3-methoxyacrylic acid, 20 g of isobutyl cinnamate, 30 g of docosyl methacrylate, 0.6 g of azobisisobutyronitrile and 90 g of butyl acetate were mixed and stirred to form a monomer initiator mixture at a stirring speed of 200 r / min;
[0056] Step 3: Add the prepared monomer-initiator mixed solution to the reaction vessel through a constant pressure dropping funnel. The dropping time is 3 hours. After the dropping is completed, keep warm for 1.5 hours.
[0057] Step 4: 0.2 g of azobisisobutyronitrile and 10 g of butyl acetate were mixed and stirred to form an initiator mixture, and the initiator mixture solution was added dropwise to the reaction container to initiate polymerization of the remaining monomers. The stirring speed was 200 r / min and the dropping time was 15 min.
[0058] Step 5: After the initiator mixed solution is added dropwise, keep the mixture warm for 1.5 hours, and stir and cool to room temperature to obtain a high-viscosity / degradable acrylic pressure-sensitive adhesive.
[0059] Example 4
[0060] Step 1: Place 110 g of ethyl propionate into a reaction vessel, heat to 85°C, and introduce nitrogen protection;
[0061] Step 2: 30 g of prop-2-en-1-ylcarbamate, 45 g of 4-methyl-1,2-dithiolane-4-carboxylic acid, 2 g of 3-methoxyacrylic acid, 30 g of isobutyl cinnamate, 40 g of behenyl methacrylate, 0.4 g of dibenzoyl peroxide and 110 g of ethyl propionate are mixed and stirred to form a monomer hair dryer mixture at a stirring speed of 200 r / min;
[0062] Step 3: Add the prepared monomer-initiator mixed solution to the reaction vessel through a constant pressure dropping funnel. The dropping time is 4 hours. After the dropping is completed, keep warm for 1.5 hours.
[0063] Step 4: 0.2 g of dibenzoyl peroxide and 10 g of ethyl propionate were mixed and stirred to form an initiator mixed solution, and the initiator mixed solution was added dropwise to the reaction container to initiate polymerization of the remaining monomers. The stirring speed was 200 r / min and the dropping time was 15 min.
[0064] Step 5: After the initiator mixed solution is added dropwise, keep the mixture warm for 1.5 hours, and stir and cool to room temperature to obtain a high-viscosity / degradable acrylic pressure-sensitive adhesive.
[0065] Example 5
[0066] Step 1: 110 g of propyl acetate was placed in a reaction vessel, the temperature was raised to 90°C, and nitrogen was introduced for protection;
[0067] Step 2: 35 g of prop-2-en-1-ylcarbamate, 60 g of 4-methyl-1,2-dithiolane-4-carboxylic acid, 3 g of 3-methoxyacrylic acid, 25 g of isobutyl cinnamate, 40 g of behenyl methacrylate, 0.4 g of dibenzoyl peroxide and 110 g of propyl acetate were mixed and stirred to form a monomer initiator mixture at a stirring speed of 200 r / min;
[0068] Step 3: Add the prepared monomer-initiator mixed solution to the reaction vessel through a constant pressure dropping funnel. The dropping time is 1.5 hours. After the dropping is completed, keep warm for 1.5 hours;
[0069] Step 4: 0.1 g of dibenzoyl peroxide and 10 g of ethyl propionate were mixed and stirred to form an initiator mixed solution, and the initiator mixed solution was added dropwise to the reaction container to initiate polymerization of the remaining monomers. The stirring speed was 200 r / min and the dropping time was 15 min.
[0070] Step 5: After the initiator mixed solution is added dropwise, keep the mixture warm for 1.5 hours, and stir and cool to room temperature to obtain a high-viscosity / degradable acrylic pressure-sensitive adhesive.
[0071] Example 6
[0072] Step 1: Place 90 g of toluene into a reaction vessel, heat to 95°C, and introduce nitrogen protection;
[0073] Step 2: 30 g of prop-2-en-1-ylcarbamate, 55 g of 4-methyl-1,2-dithiolane-4-carboxylic acid, 3 g of 3-methoxyacrylic acid, 25 g of isobutyl cinnamate, 45 g of behenyl methacrylate, 0.4 g of tert-butyl peroxyvalerate and 90 g of toluene are mixed and stirred to form a monomer initiator mixture at a stirring speed of 200 r / min;
[0074] Step 3: Add the prepared monomer-initiator mixed solution to the reaction vessel through a constant pressure dropping funnel for 3.5 hours, and keep warm for 1.5 hours after the addition is completed;
[0075] Step 4: 0.1 g of tert-butyl peroxyvalerate and 10 g of toluene were mixed and stirred to form an initiator mixed solution, and the initiator mixed solution was added dropwise to the reaction container to initiate polymerization of the remaining monomers. The stirring speed was 200 r / min and the dropping time was 15 min.
[0076] Step 5: After the initiator mixed solution is added dropwise, keep the mixture warm for 1.5 hours, and stir and cool to room temperature to obtain a high-viscosity / degradable acrylic pressure-sensitive adhesive.
[0077] Comparative Example 1
[0078] Step 1: Place 60 g of ethyl propionate into a reaction vessel, heat to 85°C, and introduce nitrogen protection;
[0079] Step 2: 30 g of prop-2-en-1-yl carbamate, 3 g of 3-methoxyacrylic acid, 25 g of isobutyl cinnamate, 45 g of behenyl methacrylate, 0.4 g of dibenzoyl peroxide and 60 g of ethyl propionate were mixed and stirred to form a monomer initiator mixture at a stirring speed of 200 r / min;
[0080] Step 3: Add the prepared monomer-initiator mixed solution to the reaction vessel through a constant pressure dropping funnel. The dropping time is 4 hours. After the dropping is completed, keep warm for 1.5 hours.
[0081] Step 4: Mix 0.1 g of dibenzoyl peroxide and 10 g of ethyl propionate and stir them evenly to form an initiator mixed solution, and drop the initiator mixed solution into the reaction container to initiate polymerization of the remaining monomers. The stirring speed is 200 r / min and the dropping time is 15 min.
[0082] Step 5: After the initiator mixed solution is added dropwise, keep the mixture warm for 1.5 hours, and stir and cool to room temperature to obtain a high-viscosity / degradable acrylic pressure-sensitive adhesive.
[0083] Comparative Example 2
[0084] Step 1: Place 60 g of toluene into a reaction vessel, heat to 75°C, and introduce nitrogen protection;
[0085] Step 2: 35 g of n-octyl acrylate, 5 g of acrylic acid, 25 g of methyl methacrylate, 40 g of n-butyl acrylate, 0.4 g of tert-butyl peroxyvalerate, 0.4 g of dodecyl peroxide and 60 g of toluene are mixed and stirred to form a monomer initiator at a stirring speed of 200 r / min;
[0086] Step 3: Add the prepared monomer-initiator mixed solution to the reaction vessel through a constant pressure dropping funnel. The dropping time is 3 hours. After the dropping is completed, keep warm for 1.5 hours.
[0087] Step 4: 0.1 g of dodecyl peroxide and 10 g of toluene were mixed evenly to form an initiator mixed solution, and the initiator mixed solution was added dropwise to the reaction container to initiate polymerization of the remaining monomers, with a stirring speed of 200 r / min and a dropping time of 15 min;
[0088] Step 5: After the initiator mixed solution is added dropwise, keep the mixture warm for 1.5 hours, and stir and cool to room temperature to obtain a high-viscosity / degradable acrylic pressure-sensitive adhesive.
[0089] Comparative Example 3
[0090] Step 1: Place 80 g of butyl acetate into a reaction vessel and heat to 75°C. Pass nitrogen gas for protection;
[0091] Step 2: 65 g of n-butyl acrylate, 5 g of acrylic acid, 25 g of methyl methacrylate, 30 g of cyclohexyl acrylate, 0.5 g of azobisisobutyronitrile, 0.2 g of azobisisobutyronitrile and 80 g of butyl acetate were mixed and stirred to form a monomer initiator mixture at a stirring speed of 200 r / min;
[0092] Step 3: Add the prepared monomer-initiator mixed solution to the reaction vessel through a constant pressure dropping funnel. The dropping time is 3 hours. After the dropping is completed, keep warm for 1.5 hours.
[0093] Step 4: 0.1 g of azobisisobutyronitrile and 10 g of butyl acetate were mixed to form an initiator mixture, and the initiator mixture solution was added dropwise to the reaction container to initiate polymerization of the remaining monomers. The stirring speed was 200 r / min and the dropping time was 15 min.
[0094] Step 5: After the initiator mixed solution is added dropwise, keep the mixture warm for 1.5 hours, and stir and cool to room temperature to obtain a high-viscosity / degradable acrylic pressure-sensitive adhesive.
[0095] The performance tests of the high-viscosity, degradable acrylate pressure-sensitive adhesive and the preparation method thereof obtained in Examples 1 to 6 and Comparative Examples 1 to 3 were performed, and the results are shown in the following table:
[0096]
[0097]
[0098] 1. Gel Permeation Chromatography (GPC)
[0099] At 30 °C, tetrahydrofuran was used as the eluent with a flow rate of 1.0 ml min -1 The number average relative molecular mass Mn was determined by gel permeation chromatography (GPC), and the relative molecular mass was calculated based on the calibration curve calibrated by standard polystyrene.
[0100] 2.180° peeling force
[0101] According to the standard GB / T2792-2014, the samples were subjected to a 180° peel force test. The coated samples were subjected to a 180° peel test using an electronic peel tester (ChemInstruments, USA). The strips were cut into 25mm*200mm strips. These strips were removed from the release liner and applied to a standard test plate. The rolling was repeated 3 times with a 2.5 kg roller, and then pulled out from the standard test plate at a speed of 180° at a speed of 300 mm / min.
[0102] 3. Ring initial adhesion
[0103] The temperature is 23℃±2℃, the humidity is 50%RH±5%RH, and the test specimen should be placed for at least 4 hours before testing. Five specimens with a width of 25mm and a length of at least 175mm were cut for testing. Before testing, the backing of the tape was removed, the adhesive surface was facing outward, and the two ends of the tape were held to form a ring. The end of the ring was clamped into the upper fixture of the tensile machine 10mm away, and the ring drooped vertically. The glass plate was clamped into the lower fixture, and its radial direction was perpendicular to the radial direction of the tape. The ring was brought into contact with the glass plate at a speed of 300mm / min. After contact, it was immediately separated in the opposite direction at a speed of 300mm / min. The important point is to make the reverse separation lag time as short as possible, and record the maximum force value for separating the ring and the glass plate.
[0104] 4. Degradability: The tapes of the embodiments and comparative examples were cut into 5 specimens of 15 cm in length and 10 cm in width, and the mass m0 before degradation was weighed first. The specimens were immersed in a phosphate solution containing 20 mmol / L mercaptoethanol at a pH of about 7 and sealed for 7 days. The mass m1 after degradation was weighed again. The decomposition rate = (m0-m1) / m0*100%.
[0105] 5. Weather resistance: The adhesive tapes of the embodiments and comparative examples were cut into 5 samples each with a length of 15 cm and a width of 25 mm. The adhesive test was carried out at a temperature of 23°C ± 2°C and a humidity of 50% RH ± 5% RH.
[0106] It can be seen from the results in the above table that the prepared high-viscosity, degradable acrylate pressure-sensitive adhesive has good bonding ability and degradation ability. In Example 2, the content of disulfide heterocyclic monomer is high and the degradation ability is good, but the bonding ability is limited. In Example 1, the content of dioctyl methacrylate is high and the bonding ability is excellent, but the degradation ability is deteriorated. In Example 5 and Example 6, the content of dioctyl methacrylate and disulfide heterocyclic monomer is the preferred value. The results show that the comprehensive effect of bonding ability and degradation ability is the most excellent. And the introduction of degradable cyclic monomers does not affect the weather resistance of acrylate pressure-sensitive adhesive. The present invention provides a new preparation process for the application of acrylate pressure-sensitive adhesive, and the prepared high-viscosity, degradable acrylate pressure-sensitive adhesive meets the use requirements of bonding and expands the application field of acrylate pressure-sensitive adhesive.
[0107] It should be noted that in the above embodiments, as long as the technical solutions are not contradictory, they can be arranged and combined, and those skilled in the art can exhaust all possibilities based on the mathematical knowledge of arrangement and combination. Therefore, the present invention will no longer describe the technical solutions after arrangement and combination one by one, but it should be understood that the technical solutions after arrangement and combination have been disclosed by the present invention.
[0108] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A high-viscosity / degradable acrylic pressure-sensitive adhesive, characterized in that: The high-viscosity / degradable acrylic pressure-sensitive adhesive is composed of prop-2-en-1-yl carbamate, 4-methyl-1.2-dithiolane-4-carboxylic acid, 3-methoxyacrylic acid, isobutyl cinnamate, behenyl methacrylate, a thermal initiator, and a solvent; The mass fraction of prop-2-en-1-ylcarbamate is 20-40 parts, the mass fraction of 4-methyl-1,2-dithiolane-4-carboxylic acid is 30-80 parts, the mass fraction of 3-methoxyacrylic acid is 1-5 parts, the mass fraction of isobutyl cinnamate is 20-30 parts, the mass fraction of behenyl methacrylate is 30-60 parts, the mass fraction of thermal initiator is 0.3-0.8 parts, and the mass fraction of solvent is 190-300 parts.
2. A high viscosity / degradable acrylic pressure-sensitive adhesive according to claim 1, characterized in that: The thermal initiator is one or more of benzoyl peroxide, tert-butyl peroxyvalerate, azobisisobutyronitrile, or dodecanoyl peroxide.
3. The high-viscosity / degradable acrylic pressure-sensitive adhesive according to claim 1, characterized in that: The solvent is one or more of toluene, butyl acetate, propyl acetate and ethyl propionate.
4. A method for preparing a high-viscosity / degradable acrylic pressure-sensitive adhesive, characterized in that: The steps include: Step 1: Put part of the solvent into a reaction container, heat the reaction container, and introduce nitrogen protection after heating; Step 2: Propylene-2-en-1-ylcarbamate, 4-methyl-1,2-dithiolane-4-carboxylic acid, 3-methoxyacrylic acid, isobutyl cinnamate, docosyl methacrylate, part of the thermal initiator and part of the solvent are mixed and stirred to obtain a monomer initiator mixed solution; Step 3: Add the monomer-initiator mixed solution dropwise to the reaction container, and keep warm after the addition is completed; Step 4: Mix the thermal initiator and the solution and stir them evenly to obtain an initiator mixed solution, and drop the initiator mixed solution into the reaction container; Step 5: After the initiator mixed solution is added dropwise, the mixture is kept warm, stirred and cooled to room temperature to obtain a high viscosity / degradable acrylic pressure-sensitive adhesive.
5. A method for preparing a high-viscosity / degradable acrylic pressure-sensitive adhesive according to claim 4, characterized in that: The stirring rate is 150-200 r / min, and the temperature of the reaction container in step 1 is raised to 75-95°C.
6. A method for preparing a high-viscosity / degradable acrylic pressure-sensitive adhesive according to claim 4, characterized in that: The insulation time is 1.5h.
7. A method for preparing a high-viscosity / degradable acrylic pressure-sensitive adhesive according to claim 4, characterized in that: In the step 3, the monomer-initiator mixed solution is added dropwise to the reaction container through a constant pressure dropping funnel, and the adding time is 1-6 hours. In the step 4, the adding time is 15 minutes.
Citation Information
Cited By
Biodegradable resin type pressure-sensitive adhesive
CN120484728A
High-wear-resistance tire material, preparation method thereof and tire
CN122381574A