Preparation method of bio-based high-frequency assembly adhesive

By grinding and drying crude lignin, combined with polyvinyl alcohol and crosslinking agent, microwave and graphene oxide intervention were used to prepare bio-based high-frequency assembly glue, which solved the problem of poor initial viscosity of lignin and improved the glue The heat and water resistance performance meets the needs of high-frequency assembly of adhesives and realizes the development of green and environmentally friendly adhesives.

CN118931438APending Publication Date: 2024-11-12DINGLI NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411272486.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-11
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The main raw materials of existing adhesives are reduced, and the initial viscosity of lignin is poor, making it difficult to widely use in adhesives. The traditional hot pressing mode is inefficient and cannot meet the needs of high-frequency hot pressing.

Method used

By grinding and drying crude lignin, combining polyvinyl alcohol and crosslinking agent, microwave and graphene oxide intervention, the initial adhesion and bonding strength of lignin are enhanced, and biological preparation is prepared through specific reaction steps and additive adjustments. Base high frequency assembly glue.

Benefits of technology

It significantly improves the initial adhesion and bonding strength of lignin, improves the heat and water resistance of glue, meets the needs of high-frequency assembly of glue, and meets green and environmentally friendly standards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention discloses a preparation method of a bio-based high-frequency assembly adhesive, and particularly relates to the technical field of formaldehyde-free bio-based adhesive processing. According to the invention, modified lignin is selected as a raw material, and modified lignin with excellent performance is prepared by crosslinking modification of lignin and polyvinyl alcohol; the initial adhesion of the modified lignin and the number of polar groups are obviously improved, and the improvement of high-frequency strength is facilitated; graphene oxide is grafted in the emulsion polymerization process to form a type reinforcing steel bar structure, so that the water resistance and heat resistance of the glue are further enhanced; the problem that existing high-frequency glue is insufficient in water resistance at present is solved, and the glue can be rapidly cured to form strength by increasing polar groups of the glue. The preparation method is simple and easy to operate, can reduce the use of petroleum derivatives, is safe and environment-friendly, and also can reduce the production cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of formaldehyde-free bio-based adhesives, and in particular relates to a method for preparing a bio-based high-frequency assembly adhesive. Background Art

[0002] With the progress and development of society, people are also demanding further improvement in productivity; high-frequency hot pressing has obvious advantages over traditional hot pressing; when high-frequency current passes through the induction coil, the internal magnetic field of the induction coil will change accordingly, causing the internal molecules to move violently with the change of the magnetic field, thereby forming heat energy; compared with the traditional heat conduction mode, it is more efficient and energy-saving; and the flatness of the boards produced by high-frequency paneling is very good, which is in line with the consumption concepts of modern consumers; the high-frequency paneling machine has brought significant benefits and cost savings to the production of home furniture through its high efficiency, high flatness, high stability, wide applicability and energy-saving and environmental protection.

[0003] The times are progressing and developing. However, coal and oil, which are the main sources of raw materials for adhesives at this stage, are decreasing day by day, and people are calling for renewable and green materials more and more. Lignin is widely found in various plants and contains a large number of active groups. It is very suitable as a raw material for adhesives. However, it is not widely used in adhesives due to its poor initial adhesion and high hot pressing temperature. Therefore, the modification of lignin is a development trend. The cross-linking agent is used to graft polyvinyl alcohol onto lignin to make up for the disadvantages of lignin itself. Moreover, lignin itself has many polar groups, and the molecules vibrate violently under the action of microwaves, which effectively increases the heating rate of the glue itself and improves production efficiency. The intervention of graphene oxide can effectively improve the quality of production products and significantly improve the bonding strength and heat and water resistance of the glue. Summary of the invention

[0004] The purpose of the present invention is to provide a method for preparing a bio-based high-frequency assembly adhesive in view of the deficiencies of the prior art.

[0005] The object of the present invention is achieved through the following technical scheme: A method for preparing a bio-based high-frequency assembly adhesive comprises the following steps:

[0006] (1) Grinding the crude lignin with a grinder for 1 to 2 hours, then adding water to fully dissolve it, filtering it evenly through a 400-mesh sieve, taking the filtrate and putting it in a 60° C. oven for 3 to 12 hours, and drying it until the moisture content is less than 5 wt % to obtain refined lignin;

[0007] (2) adding 100 to 300 parts by weight of refined lignin, 50 to 100 parts by weight of polyvinyl alcohol and 700 to 1000 parts by weight of water into a reaction kettle, heating the reaction kettle to 80 to 95° C., and keeping the temperature for 30 to 120 minutes;

[0008] (3) After cooling the reactor to 50-70° C., 0.5-2 parts by weight of an acid solution and 3-8 parts by weight of a cross-linking agent are added, and then the temperature is raised to 70-80° C. for a reaction time of 30-120 min;

[0009] (4) After the reaction is completed, 0.5 to 1 parts by weight of an alkaline solution is added to adjust the pH to 5.0 to 7.0, and then 0.5 to 2 parts by weight of an emulsifier is added and emulsified for 10 to 20 minutes;

[0010] (5) After the emulsification is completed, 30 to 60 parts by weight of the first monomer and 1 to 2 parts by weight of the initiator solution are added to the reactor and kept warm for 40 to 80 minutes;

[0011] (6) 300-400 parts by weight of the first monomer, 20-40 parts by weight of the second monomer, and 5-20 parts by weight of the enhancer are uniformly stirred, and are simultaneously dripped into the reaction kettle with 3-10 parts by weight of the initiator solution, at a temperature of 76-82° C. for 3-5 hours; after the dripping is completed, the temperature is raised to 85-92° C., and then 0.5-1 parts by weight of the initiator solution is added, and the temperature is kept at 60-90 minutes;

[0012] (7) The temperature is then lowered to below 50° C., and 0.5 to 2 parts by weight of a mildew inhibitor is added to the reaction kettle. The mixture is stirred for 30 minutes to obtain a finished emulsion, which is a bio-based high-frequency assembly adhesive.

[0013] Furthermore, the polyvinyl alcohol is composed of one or more of VA1788, PVA0588, PVA2488, and PVA0488 mixed in any proportion.

[0014] Furthermore, the acid solution is composed of one or both of 5-30wt% hydrogen chloride solution and dilute sulfuric acid solution mixed in any ratio.

[0015] Furthermore, the cross-linking agent is one or more of butyraldehyde, glutaraldehyde, succinaldehyde, and aziridine cross-linking agents mixed in any proportion.

[0016] Furthermore, the alkaline solution is composed of one or more of 5-30wt% ammonia solution, sodium bicarbonate solution, and sodium hydroxide solution mixed in any proportion.

[0017] Furthermore, the emulsifier is composed of one or more of OP-10, ER-10, ER-20, and SR-10 mixed in any ratio.

[0018] Furthermore, the first monomer is polyvinyl acetate with a mass fraction greater than 99 wt%.

[0019] Furthermore, the second monomer is one or more of acrylic acid, hydroxypropyl acrylate, and hydroxyethyl acrylate mixed in any proportion.

[0020] Furthermore, the reinforcing agent is a mixture of one or both of multilayer graphene oxide and single layer graphene oxide in any ratio.

[0021] Furthermore, the initiator solution is composed of one or both of an ammonium persulfate solution and a potassium persulfate solution with a concentration of 1 to 5 wt % and mixed in any ratio.

[0022] Furthermore, the mildew preventer is composed of one or more of 1,2-benzisothiazolin-3-one, 2-methyl-4-isothiazolin-3-one, and chloromethylisothiazolinone mixed in any proportion.

[0023] The beneficial effects of the present invention are:

[0024] 1) This invention abandons the mainstream petroleum products and adds a large amount of renewable lignin; and uses polyvinyl alcohol to modify lignin, which greatly improves the initial adhesion and bonding strength of lignin, making lignin more widely used in high-frequency glue;

[0025] 2) The invention introduces graphene oxide during polymerization, and through graft copolymerization, the overall tensile properties of the polymer chain segment are improved, further improving the quality of the product, and improving the bonding strength and heat and water resistance of the product;

[0026] 3) The cross-linking agent used in this product can effectively enhance the cross-linking between lignin and polyvinyl alcohol, and will not produce harmful substances such as formaldehyde during the reaction, which is in line with the concept of green and environmental protection. DETAILED DESCRIPTION

[0027] In order to make the purpose, technical scheme and advantages of the present invention more clear, the present invention is further described in detail in combination with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention, rather than all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0028] The present invention provides a method for preparing a bio-based high-frequency assembly adhesive, comprising the following steps:

[0029] (1) Grinding the crude lignin with a grinder for 1 to 2 hours, then adding water to fully dissolve it, filtering it evenly through a 400-mesh sieve, taking the filtrate and putting it in a 60° C. oven for 3 to 12 hours, and drying it until the moisture content is less than 5 wt % to obtain refined lignin;

[0030] (2) adding 100 to 300 parts by weight of refined lignin, 50 to 100 parts by weight of polyvinyl alcohol and 700 to 1000 parts by weight of water into a reaction kettle, heating the reaction kettle to 80 to 95° C., and keeping the temperature for 30 to 120 minutes;

[0031] (3) After cooling the reactor to 50-70° C., 0.5-2 parts by weight of an acid solution and 3-8 parts by weight of a cross-linking agent are added, and then the temperature is raised to 70-80° C. for a reaction time of 30-120 min;

[0032] (4) After the reaction is completed, 0.5 to 1 parts by weight of an alkaline solution is added to adjust the pH to 5.0 to 7.0, and then 0.5 to 2 parts by weight of an emulsifier is added and emulsified for 10 to 20 minutes;

[0033] (5) After the emulsification is completed, 30 to 60 parts by weight of the first monomer and 1 to 2 parts by weight of the initiator solution are added to the reactor and kept warm for 40 to 80 minutes;

[0034] (6) 300-400 parts by weight of the first monomer, 20-40 parts by weight of the second monomer, and 5-20 parts by weight of the enhancer are uniformly stirred, and are simultaneously dripped into the reaction kettle with 3-10 parts by weight of the initiator solution, at a temperature of 76-82° C. for 3-5 hours; after the dripping is completed, the temperature is raised to 85-92° C., and then 0.5-1 parts by weight of the initiator solution is added, and the temperature is kept at 60-90 minutes;

[0035] (7) The temperature is then lowered to below 50° C., and 0.5 to 2 parts by weight of a mildew inhibitor is added to the reaction kettle. The mixture is stirred for 30 minutes to obtain a finished emulsion, which is a bio-based high-frequency assembly adhesive.

[0036] The polyvinyl alcohol is composed of one or more of VA1788, PVA0588, PVA2488 and PVA0488 mixed in any proportion.

[0037] The acid solution is composed of a mixture of 5-30wt% hydrogen chloride solution and dilute sulfuric acid solution or both in any proportion.

[0038] The cross-linking agent is one or more of butyraldehyde, glutaraldehyde, succinaldehyde and aziridine cross-linking agents mixed in any proportion.

[0039] The alkaline solution is a mixture of one or more of 5-30wt% ammonia solution, sodium bicarbonate solution and sodium hydroxide solution in any proportion.

[0040] The emulsifier is one or more of OP-10, ER-10, ER-20 and SR-10 mixed in any proportion.

[0041] The first monomer is polyvinyl acetate with a mass fraction greater than 99wt%.

[0042] The second monomer is one or more of acrylic acid, hydroxypropyl acrylate and hydroxyethyl acrylate mixed in any proportion.

[0043] The reinforcing agent is a mixture of one or both of multilayer graphene oxide and single layer graphene oxide in any proportion.

[0044] The initiator solution is composed of one or both of an ammonium persulfate solution and a potassium persulfate solution with a concentration of 1-5 wt % and mixed in any proportion.

[0045] The mildew preventer is composed of one or more of 1,2-benzisothiazolin-3-one, 2-methyl-4-isothiazolin-3-one and chloromethylisothiazolinone mixed in any proportion.

[0046] Example 1

[0047] (1) The crude lignin was ground using a grinder for 1 h, then water was added to fully dissolve it, and after it was evenly distributed, it was filtered through a 400-mesh sieve. The filtrate was placed in a 60° C. oven for 6 h and dried to a moisture content of 4 wt % to obtain refined lignin.

[0048] (2) 200 parts by weight of refined lignin, 50 parts by weight of VA1788 and 800 parts by weight of water were added into a reactor, and the temperature was raised to 90° C. and kept at this temperature for 60 min.

[0049] (3) The reaction kettle was then cooled to 60° C., 0.5 parts by weight of 8 wt % hydrogen chloride solution and 4 parts by weight of glutaraldehyde were added, and then the temperature was slowly raised to 75° C. The reaction time was 60 min.

[0050] (4) After the reaction was completed, 0.5 parts by weight of 28 wt% ammonia solution was added to the reactor to adjust the pH to 7, and then 1 part by weight of OP-10 was added and emulsified for 10 minutes.

[0051] (5) After the emulsification is completed, 50 parts by weight of polyvinyl acetate with a mass fraction greater than 99 wt% and 1 part by weight of ammonium persulfate solution with a concentration of 2 wt% are added to the reactor and maintained for 60 minutes.

[0052] (6) 350 parts by weight of polyvinyl acetate with a mass fraction greater than 99 wt%, 20 parts by weight of acrylic acid, and 5 parts by weight of single-layer graphene oxide were uniformly stirred, and added dropwise into the reactor simultaneously with 5 parts by weight of a 2 wt% ammonium persulfate solution, the dropping temperature was 78°C, and the dropping time was 4 h; after the dropping was completed, the temperature was raised to 90°C, and then 0.5 parts by weight of a 2 wt% ammonium persulfate solution was added, and the temperature was kept warm for 70 min.

[0053] (7) The temperature was then lowered to 50° C., and 1 part by weight of 1,2-benzisothiazolin-3-one was added to the reaction kettle, and stirred for 30 minutes to obtain a finished emulsion, which was a bio-based high-frequency assembly adhesive.

[0054] Example 2

[0055] A method for preparing a bio-based high-frequency assembly adhesive comprises the following steps:

[0056] (1) The crude lignin was ground using a grinder for 1 h, then water was added to fully dissolve it, and after it was evenly distributed, it was filtered through a 400-mesh sieve. The filtrate was placed in a 60° C. oven for 6 h and dried to a moisture content of 4 wt % to obtain refined lignin.

[0057] (2) 200 parts by weight of refined lignin, 50 parts by weight of VA1788 and 800 parts by weight of water were added into a reactor, and the temperature was raised to 90° C. and kept at this temperature for 60 min.

[0058] (3) The reaction kettle was then cooled to 60° C., 0.5 parts by weight of 8 wt % hydrogen chloride solution and 4 parts by weight of glutaraldehyde were added, and then the temperature was slowly raised to 75° C. The reaction time was 60 min.

[0059] (4) After the reaction was completed, 0.5 parts by weight of 28 wt% ammonia solution was added to the reactor to adjust the pH to 7, and then 1 part by weight of OP-10 was added and emulsified for 10 minutes.

[0060] (5) After the emulsification is completed, 50 parts by weight of polyvinyl acetate with a mass fraction greater than 99 wt% and 1 part by weight of ammonium persulfate solution with a concentration of 2 wt% are added to the reactor and maintained for 60 minutes.

[0061] (6) 350 parts by weight of polyvinyl acetate with a mass fraction greater than 99 wt%, 20 parts by weight of acrylic acid, and 15 parts by weight of single-layer graphene oxide were stirred evenly, and added dropwise into the reactor simultaneously with 5 parts by weight of a 2 wt% ammonium persulfate solution, the dropping temperature was 78°C, and the dropping time was 4 h; after the dropping was completed, the temperature was raised to 90°C, and then 0.5 parts by weight of a 2 wt% ammonium persulfate solution was added, and the mixture was kept warm for 70 min.

[0062] (7) The temperature was then lowered to 50° C., and 1 part by weight of 1,2-benzisothiazolin-3-one was added to the reaction kettle, and stirred for 30 minutes to obtain a finished emulsion, which was a bio-based high-frequency assembly adhesive.

[0063] Example 3

[0064] A method for preparing a bio-based high-frequency assembly adhesive comprises the following steps:

[0065] (1) The crude lignin was ground using a grinder for 1 h, then water was added to fully dissolve it, and after it was evenly distributed, it was filtered through a 400-mesh sieve. The filtrate was placed in a 60° C. oven for 6 h and dried to a moisture content of 4 wt % to obtain refined lignin.

[0066] (2) 300 parts by weight of refined lignin, 50 parts by weight of VA1788 and 800 parts by weight of water were added into a reactor, and the temperature was raised to 90° C. and kept at this temperature for 60 min.

[0067] (3) The reaction kettle was then cooled to 60° C., 0.5 parts by weight of 8 wt % hydrogen chloride solution and 4 parts by weight of glutaraldehyde were added, and then the temperature was slowly raised to 75° C. The reaction time was 60 min.

[0068] (4) After the reaction was completed, 0.5 parts by weight of 28 wt% ammonia solution was added to the reactor to adjust the pH to 7, and then 1 part by weight of OP-10 was added and emulsified for 10 minutes.

[0069] (5) After the emulsification is completed, 50 parts by weight of polyvinyl acetate with a mass fraction greater than 99 wt% and 1 part by weight of ammonium persulfate solution with a concentration of 2 wt% are added to the reactor and maintained for 60 minutes.

[0070] (6) 350 parts by weight of polyvinyl acetate with a mass fraction greater than 99 wt%, 20 parts by weight of acrylic acid, and 5 parts by weight of single-layer graphene oxide were uniformly stirred, and added dropwise into the reactor simultaneously with 5 parts by weight of a 2 wt% ammonium persulfate solution, the dropping temperature was 78°C, and the dropping time was 4 h; after the dropping was completed, the temperature was raised to 90°C, and then 0.5 parts by weight of a 2 wt% ammonium persulfate solution was added, and the temperature was kept warm for 70 min.

[0071] (7) The temperature was then lowered to 50° C., and 1 part by weight of 1,2-benzisothiazolin-3-one was added to the reaction kettle, and stirred for 30 minutes to obtain a finished emulsion, which was a bio-based high-frequency assembly adhesive.

[0072] Example 4

[0073] A method for preparing a bio-based high-frequency assembly adhesive comprises the following steps:

[0074] (1) The crude lignin was ground using a grinder for 1 h, then water was added to fully dissolve it, and after it was evenly distributed, it was filtered through a 400-mesh sieve. The filtrate was placed in a 60° C. oven for 6 h and dried to a moisture content of 4 wt % to obtain refined lignin.

[0075] (2) 200 parts by weight of refined lignin, 50 parts by weight of VA1788 and 800 parts by weight of water were added into a reactor, and the temperature was raised to 90° C. and kept at this temperature for 60 min.

[0076] (3) The reaction kettle was then cooled to 60° C., 0.5 parts by weight of 8 wt % hydrogen chloride solution and 4 parts by weight of an aqueous aziridine crosslinking agent were added, and then the temperature was slowly raised to 75° C. The reaction time was 60 min.

[0077] (4) After the reaction was completed, 0.5 parts by weight of 28 wt% ammonia solution was added to the reactor to adjust the pH to 7, and then 1 part by weight of OP-10 was added and emulsified for 10 minutes.

[0078] (5) After the emulsification is completed, 50 parts by weight of polyvinyl acetate with a mass fraction greater than 99 wt% and 1 part by weight of ammonium persulfate solution with a concentration of 2 wt% are added to the reactor and maintained for 60 minutes.

[0079] (6) 350 parts by weight of polyvinyl acetate with a mass fraction greater than 99 wt%, 20 parts by weight of acrylic acid, and 5 parts by weight of single-layer graphene oxide were uniformly stirred, and added dropwise into the reactor simultaneously with 5 parts by weight of a 2 wt% ammonium persulfate solution, the dropping temperature was 78°C, and the dropping time was 4 h; after the dropping was completed, the temperature was raised to 90°C, and then 0.5 parts by weight of a 2 wt% ammonium persulfate solution was added, and the temperature was kept warm for 70 min.

[0080] (7) The temperature was then lowered to 50° C., and 1 part by weight of 1,2-benzisothiazolin-3-one was added to the reaction kettle, and stirred for 30 minutes to obtain a finished emulsion, which was a bio-based high-frequency assembly adhesive.

[0081] Example 5

[0082] A method for preparing a bio-based high-frequency assembly adhesive comprises the following steps:

[0083] (1) The crude lignin was ground using a grinder for 1 h, then water was added to fully dissolve it, and after it was evenly distributed, it was filtered through a 400-mesh sieve. The filtrate was placed in a 60° C. oven for 6 h and dried to a moisture content of 4 wt % to obtain refined lignin.

[0084] (2) 200 parts by weight of refined lignin, 50 parts by weight of VA1788 and 800 parts by weight of water were added into a reactor, and the temperature was raised to 90° C. and kept at this temperature for 60 min.

[0085] (3) The reaction kettle was then cooled to 60° C., 0.5 parts by weight of 8 wt % hydrogen chloride solution and 6 parts by weight of glutaraldehyde were added, and then the temperature was slowly raised to 75° C. The reaction time was 60 min.

[0086] (4) After the reaction was completed, 0.5 parts by weight of 28 wt% ammonia solution was added to the reactor to adjust the pH to 7, and then 1 part by weight of OP-10 was added and emulsified for 10 minutes.

[0087] (5) After the emulsification is completed, 50 parts by weight of polyvinyl acetate with a mass fraction greater than 99 wt% and 1 part by weight of ammonium persulfate solution with a concentration of 2 wt% are added to the reactor and maintained for 60 minutes.

[0088] (6) 350 parts by weight of polyvinyl acetate with a mass fraction greater than 99 wt%, 20 parts by weight of acrylic acid, and 5 parts by weight of single-layer graphene oxide were uniformly stirred, and added dropwise into the reactor simultaneously with 5 parts by weight of a 2 wt% ammonium persulfate solution, the dropping temperature was 78°C, and the dropping time was 4 h; after the dropping was completed, the temperature was raised to 90°C, and then 0.5 parts by weight of a 2 wt% ammonium persulfate solution was added, and the temperature was kept warm for 70 min.

[0089] (7) The temperature was then lowered to 50° C., and 1 part by weight of 1,2-benzisothiazolin-3-one was added to the reaction kettle, and stirred for 30 minutes to obtain a finished emulsion, which was a bio-based high-frequency assembly adhesive.

[0090] The difference between Example 2 and Example 1 is that during polymerization, the amount of the single-layer graphene oxide (reinforcer) changes from 5 parts by mass to 15 parts by mass.

[0091] The difference between Example 3 and Example 1 is that the amount of refined lignin is adjusted from 200 parts by mass to 300 parts by mass.

[0092] The difference between Example 4 and Example 1 is that glutaraldehyde (cross-linking agent) is adjusted to an aqueous aziridine cross-linking agent.

[0093] The difference between Example 5 and Example 1 is that the amount of glutaraldehyde (cross-linking agent) is adjusted from 4 parts by mass to 6 parts by mass.

[0094] Comparative Example 1 is 8812 high-frequency adhesive purchased on the market; Comparative Example 2 is 8274 high-frequency adhesive purchased on the market.

[0095] The bio-based high-frequency assembly adhesives prepared in Examples 1 to 5 and the emulsions prepared in Comparative Examples 1 and 2 were subjected to physical and chemical data tests, shear strength tests, and immersion peeling tests. The test results are shown in Table 1.

[0096] 1. Physical and chemical data testing:

[0097] Viscosity test conditions: 25℃ / 4# / 6R.

[0098] Stability test: The test environment is 25±2℃, humidity is 65±5%.

[0099] 2. Shear strength test:

[0100] The HGT 2727-2010 polyvinyl acetate emulsion wood adhesive standard test is used and is recorded in Table 1.

[0101] 3. Immersion stripping test

[0102] ① Specimen preparation: Prepared by high frequency machine, the frequency is set to 50-100KHz, and the curing time is set to 1min-5min.

[0103] ②Test method: Use the national standard GB / T18103-2000 to test the immersion peel strength. Place the bonded specimens at room temperature for 7 days, immerse the specimens in 70±3℃ hot water for 2 hours, take them out and dry them in a drying oven at 60℃±3℃ for 3 hours. The immersed specimens should be completely immersed in hot water.

[0104] ③Immersion standard requirements: The debonding rate of the glue layer is less than 10% and the debonding rate of a single glue line is less than one-third.

[0105] Table 1: Test results

[0106]

[0107]

[0108] The experimental results of each embodiment in Table 1 show that the bio-based high-frequency assembly adhesive of the present application has the advantages of high off-machine strength and excellent immersion peeling effect, short curing time, good water resistance, etc. It can be observed that the addition of a single layer of graphene oxide has a very obvious improvement in strength and immersion peeling effect; the selection of the cross-linking agent plays a decisive role in strength and adhesive stability;

[0109] In summary, the bio-based high-frequency assembly glue prepared by the present invention uses a cross-linking agent to graft polyvinyl alcohol onto lignin to make up for the disadvantage of poor initial adhesion of lignin itself. In addition, lignin itself has many polar groups, and the molecules vibrate violently under the action of microwaves, which effectively increases the heating rate of the glue itself and improves production efficiency. The intervention of graphene oxide can effectively improve the quality of production products and significantly improve the bonding strength and heat and water resistance of the glue. Under the joint action of the two, the high temperature resistance and water resistance are improved, and the broken material area and impregnation and stripping effect are far ahead of competing products.

[0110] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A method for preparing a bio-based high-frequency assembly adhesive, characterized in that: The following steps are involved: (1) Grinding the crude lignin with a grinder for 1 to 2 hours, then adding water to fully dissolve it, filtering it evenly through a 400-mesh sieve, taking the filtrate and putting it in a 60° C. oven for 3 to 12 hours, and drying it until the moisture content is less than 5 wt % to obtain refined lignin; (2) adding 100 to 300 parts by weight of refined lignin, 50 to 100 parts by weight of polyvinyl alcohol and 700 to 1000 parts by weight of water into a reaction kettle, heating the reaction kettle to 80 to 95° C., and keeping the temperature for 30 to 120 minutes; (3) After cooling the reactor to 50-70° C., 0.5-2 parts by weight of an acid solution and 3-8 parts by weight of a cross-linking agent are added, and then the temperature is raised to 70-80° C. for a reaction time of 30-120 min; (4) After the reaction is completed, 0.5 to 1 parts by weight of an alkaline solution is added to adjust the pH to 5.0 to 7.0, and then 0.5 to 2 parts by weight of an emulsifier is added and emulsified for 10 to 20 minutes; (5) After the emulsification is completed, 30 to 60 parts by weight of the first monomer and 1 to 2 parts by weight of the initiator solution are added to the reactor and kept warm for 40 to 80 minutes; (6) 300-400 parts by weight of the first monomer, 20-40 parts by weight of the second monomer, and 5-20 parts by weight of the enhancer are uniformly stirred, and are simultaneously dripped into the reaction kettle with 3-10 parts by weight of the initiator solution, at a temperature of 76-82° C. for 3-5 hours; after the dripping is completed, the temperature is raised to 85-92° C., and then 0.5-1 parts by weight of the initiator solution is added, and the temperature is kept at 60-90 minutes; (7) The temperature is then lowered to below 50° C., and 0.5 to 2 parts by weight of a mildew inhibitor is added to the reaction kettle. The mixture is stirred for 30 minutes to obtain a finished emulsion, which is a bio-based high-frequency assembly adhesive.

2. The method for preparing the bio-based high-frequency assembly adhesive according to claim 1, characterized in that: The polyvinyl alcohol is composed of one or more of VA1788, PVA0588, PVA2488 and PVA0488 mixed in any proportion.

3. The method for preparing the bio-based high-frequency assembly adhesive according to claim 1, characterized in that: The acid solution is composed of a 5-30wt% hydrogen chloride solution and a dilute sulfuric acid solution, or a mixture of the two in any proportion.

4. The method for preparing the bio-based high-frequency assembly adhesive according to claim 1, characterized in that: The cross-linking agent is one or more of butyraldehyde, glutaraldehyde, succinaldehyde and aziridine cross-linking agents mixed in any proportion.

5. The method for preparing the bio-based high-frequency assembly adhesive according to claim 1, characterized in that: The alkaline solution is a mixture of one or more of 5-30wt% ammonia solution, sodium bicarbonate solution and sodium hydroxide solution in any proportion.

6. The method for preparing the bio-based high-frequency assembly adhesive according to claim 1, characterized in that: The emulsifier is one or more of OP-10, ER-10, ER-20 and SR-10 mixed in any proportion.

7. The method for preparing the bio-based high-frequency assembly adhesive according to claim 1, characterized in that: The first monomer is polyvinyl acetate with a mass fraction greater than 99wt%.

8. The method for preparing the bio-based high-frequency assembly adhesive according to claim 1, characterized in that: The second monomer is one or more of acrylic acid, hydroxypropyl acrylate and hydroxyethyl acrylate mixed in any proportion.

9. The method for preparing the bio-based high-frequency assembly adhesive according to claim 1, characterized in that: The reinforcing agent is a mixture of one or both of multilayer graphene oxide and single layer graphene oxide in any proportion.

10. The method for preparing the bio-based high-frequency assembly adhesive according to claim 1, characterized in that: The initiator solution is composed of one or both of an ammonium persulfate solution and a potassium persulfate solution with a concentration of 1-5 wt % and mixed in any proportion.

11. The method for preparing the bio-based high-frequency assembly adhesive according to claim 1, characterized in that: The mildew preventer is composed of one or more of 1,2-benzisothiazolin-3-one, 2-methyl-4-isothiazolin-3-one and chloromethylisothiazolinone mixed in any proportion.