Modified phenolic resin adhesive and preparation method thereof
By using treated carbon fibers in phenolic resin adhesives to combine with lignin and adding specific coupling agents and melamine, the problems of poor toughness and toxic release of phenolic resin adhesives are solved, achieving high mechanical properties and environmental protection. Preparation of modified phenolic resin adhesive.
Patent Information
- Application Number
- CN202411314512.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-20
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-09-20
AI Technical Summary
The existing phenolic resin adhesives have poor toughness, are prone to cracks or breaks, and release toxic volatile small molecules during the curing process, affecting the environment and health. The lignin modification method has high temperature and high pressure, high energy consumption and secondary Problems caused by products.
Using organic acid-treated carbon fibers combined with lignin, using γ-aminopropyltrimethoxysilane and isopropyl titanate as coupling agents, lignin is activated to cross-link with carbon fibers through Lewis acid, and Add aqueous formaldehyde solution in batches, add melamine and antibacterial agent to prepare a modified phenolic resin adhesive.
It improves the mechanical properties, thermal stability and environmental protection properties of the resin, reduces formaldehyde release, enhances interface bonding, reduces the glass transition temperature of the material, and improves impact resistance and durability.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of adhesive preparation, and more specifically, to a modified phenolic resin adhesive and a preparation method thereof. Background Art
[0002] Phenolic resin adhesives are essential auxiliary materials for many processes and are widely used in packaging, transportation, construction, manufacturing, health care and renewable energy. They have the advantages of wear resistance, water resistance, heat resistance and good bonding performance. They are generally made by condensation of phenolic compounds such as phenol, m-diphenol, cresol, bisphenol A and aldehyde compounds such as formaldehyde, polyformaldehyde, furfural and glyoxal. Although phenolic resin adhesives have excellent performance, their toughness is poor and they are brittle. When impacted or bent, the adhesives are prone to cracking or breaking and cannot effectively absorb and disperse stress. In addition, phenolic resin adhesives release toxic volatile small molecules such as formaldehyde and phenol during the curing process. These substances not only pollute the environment, but may also cause health problems. Therefore, it has become an important development trend to seek a biomass polyphenol material with a wide source, low price and environmental protection to replace toxic petroleum-based phenol for the preparation of modified phenolic resin wood adhesives with excellent performance, low price and green environmental protection.
[0003] Among many biomass resources, lignin reserves are second only to cellulose. It is the only biomass resource in nature that can provide aromatic groups. In addition, it is cheap and biodegradable. However, lignin has a large molecular weight and high dispersion. The ortho-position of the phenolic hydroxyl group that reacts with formaldehyde in its structure is largely replaced by methoxy groups, resulting in low reaction activity and other unfavorable factors that limit its large-scale application in the production of phenolic resin adhesives. Therefore, in order to vigorously develop the industrial application of lignin in the production of phenolic resin adhesives, lignin must be modified and activated. At present, several commonly used modification methods are amination modification, oxidation modification, phenolization modification and other methods. However, each has its shortcomings: amination modification may involve toxic or volatile amines, which poses risks to the environment and health; under oxidation modification conditions, lignin is prone to excessive degradation, affecting its thermal stability and mechanical properties; and phenolization modification needs to be carried out under high temperature and high pressure, which not only has high energy consumption, but also may produce by-products, affecting the purity of the final product. Therefore, in view of the limitations of the above-mentioned modified lignin in preparing phenolic resin adhesives, how to seek more effective and mild reaction conditions and environmentally friendly modified phenolic resin adhesives is an important challenge facing the field of environmental science. Summary of the invention
[0004] In order to solve the above problems, the present invention provides a modified phenolic resin adhesive and a preparation method thereof.
[0005] In a first aspect, the present invention provides a method for preparing a modified phenolic resin adhesive, using the following technical solution: A method for preparing a modified phenolic resin adhesive comprises the following preparation steps: S1. Dispersing the carbon fiber treated with organic acid in industrial ethanol, adding a coupling agent thereto, and stirring evenly at room temperature to obtain a carbon fiber dispersion; adding lignin, the carbon fiber dispersion and Lewis acid to the mixed solvent, stirring continuously at 60-75° C. for 4-6 hours to uniformly disperse the mixture, filtering, washing and drying to obtain a functional filler; S2, dissolving phenol in tetrahydrofuran, adding melamine, sodium hydroxide and functional filler to phenol-tetrahydrofuran, stirring continuously at 80-90° C. for 1-3 h, adding the first batch of 37% formaldehyde aqueous solution, stirring continuously at 80-90° C. for 1-3 h, adding the second batch of 37% formaldehyde aqueous solution, and distilling under reduced pressure after completion of the reaction to obtain a modified phenolic resin; S3, mixing the modified phenolic resin, the antibacterial agent, the diluent, the plasticizer and the deionized water to obtain a modified phenolic resin adhesive.
[0006] Preferably, the coupling agent in step S1 is composed of γ-aminopropyltrimethoxysilane and isopropyl titanate triisostearate in a mass ratio of 16-20:1.
[0007] Preferably, the mixed solvent in step S1 consists of 2-p-chlorobenzylpyridine, 1-butyl-3-methylimidazole chloride and fumaric acid in a molar ratio of 8-12:1-3:1-3.
[0008] Preferably, the Lewis acid in step S1 is any one of ferric chloride, aluminum chloride and aluminum oxide.
[0009] Preferably, the step S2 comprises, by weight, 14-18 parts of phenol, 6-10 parts of functional fillers, 2-6 parts of melamine, 1-3 parts of sodium hydroxide, 34-38 parts of 37% formaldehyde aqueous solution and 80-100 parts of tetrahydrofuran.
[0010] Preferably, in step S3, the components by weight include 40-44 parts of modified phenolic resin, 16-20 parts of diluent, 1-3 parts of plasticizer, 1-3 parts of antibacterial agent and 80-100 parts of deionized water.
[0011] Preferably, the diluent in step S3 is at least one of isopropanol, ethanol and ethylene glycol.
[0012] Preferably, the antibacterial agent in step S3 is prepared by the following method: (1) Add citric acid and hydroquinone to a 0.01-0.1 M silver nitrate solution, stir evenly, heat to 60-80°C, and stir for 20-40 minutes to obtain a silver solution; (2) Add chitosan powder to deionized water to prepare a chitosan solution with a mass concentration of 11-15%, add geraniol and silver solution in sequence while stirring, adjust the pH to 6.0-7.0 after stirring evenly, let it stand for 3-5 hours, filter and dry to obtain the antibacterial agent.
[0013] Preferably, the plasticizer in step S3 is at least one of dioctyl phthalate, triphenyl phosphate, and dipentaerythritol ester.
[0014] In a second aspect, the present application also provides a modified phenolic resin adhesive, which adopts the following technical solution: A modified phenolic resin adhesive is prepared by the above preparation method.
[0015] In summary, the present invention has the following beneficial effects: When preparing modified phenolic resin adhesive, adding functional fillers prepared by lignin to the treated carbon fiber dispersion can play multiple roles: first, lignin, as a natural polymer, can enhance the mechanical properties and thermal stability of the resin matrix; second, through good combination with carbon fiber, it helps to form a more uniform composite material structure and improve the overall mechanical properties; in addition, the presence of lignin can also improve the processing performance of the resin and give the material certain environmental protection attributes, while lignin is a natural aromatic polymer that reduces the use of phenol. The present invention mixes γ-aminopropyl trimethoxysilane and triisostearate titanate isopropyl to prepare a coupling agent for use, wherein γ-aminopropyl trimethoxysilane can react with the hydroxyl group on the surface of the carbon fiber to form a covalent bond, and can also react with the hydroxyl group or other functional groups in the phenolic resin matrix, thereby establishing a strong chemical bond between the carbon fiber and the resin, and enhancing the interfacial bonding force of the two; triisostearate titanate isopropyl as another coupling agent can further promote the dispersion of carbon fiber in the resin matrix, prevent carbon fiber agglomeration, thereby ensuring that the composite material has a good microstructure and uniformity. The synergistic effect of the two coupling agents can not only enhance the adhesion of the interface, but also improve the overall mechanical properties of the material. The mixed solvent of the present invention is prepared by mixing 1-butyl-3-methylimidazolium chloride, fumaric acid and 2-p-chlorobenzylpyridine, wherein 1-butyl-3-methylimidazolium chloride, as an ionic liquid, has good solubility, can effectively dissolve lignin, and also helps to disperse carbon fibers, thereby ensuring the uniform mixing of the components in subsequent treatment; fumaric acid and 2-p-chlorobenzylpyridine can not only be used as solvents to assist in dissolution, but also can act as catalysts to a certain extent, promote the modification reaction of lignin, help to improve the reaction activity between lignin and other components, and thus improve the performance of the final product. By adjusting the ratio of the mixed solvent, an effective modification reaction can be achieved under milder conditions (such as 60-75°C), avoiding excessive degradation or other side reactions caused by high temperature and high pressure. The added Lewis aldehyde can activate the functional groups on the surface of lignin and carbon fibers, and promote the cross-linking reaction between them. When preparing phenolic resin, 37% formaldehyde aqueous solution is added in batches. This measure can control the gradual release of formaldehyde, which is conducive to balancing the reaction rate and preventing the reaction caused by adding a large amount of formaldehyde at one time from being too violent, so as to better control the crosslinking degree and molecular weight distribution of the resin. More importantly, adding formaldehyde in batches can improve the utilization rate of formaldehyde, reduce the content of unreacted free formaldehyde, and reduce the emission of free formaldehyde, so as to meet the requirements of environmental protection. The melamine added at the same time can participate in the synthesis of the resin as a comonomer, and the multiple active amino groups on its six-membered ring structure can cross-link with formaldehyde to enhance the heat resistance and mechanical properties of the resin. Due to the participation of melamine in the reaction, more formaldehyde can be consumed, further reducing the content of free formaldehyde in the final product, making the modified phenolic resin finally obtained more environmentally friendly.The preparation of the antibacterial agent in the technical solution of the present invention adopts a method in which silver nitrate, citric acid, hydroquinone and geraniol are added to a chitosan solution. Silver nitrate and hydroquinone have antibacterial properties, while citric acid can be used as a buffer to help maintain the pH value of the solution stable, thereby improving the effect of the antibacterial agent; geraniol, as a natural antibacterial agent, can enhance the antibacterial properties through synergistic effect with chitosan. The addition of this antibacterial agent can not only protect the modified phenolic resin adhesive from microbial contamination, but also give the finished product a certain antibacterial function, which is particularly suitable for application fields with high hygiene requirements. The plasticizer molecules added together with the antibacterial agent can be inserted between the molecular chains of the phenolic resin, weakening the attraction between molecules, thereby reducing the glass transition temperature of the material and enhancing its elasticity and impact resistance. This not only makes the phenolic resin easier to process and shape, but also improves the durability and service life of the final product. DETAILED DESCRIPTION
[0016] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0017] The experimental methods in the following examples are conventional methods unless otherwise specified, and the experimental materials used are purchased from conventional biochemical reagent stores unless otherwise specified. The quantitative tests in the following examples were repeated three times, and the data are the average or average ± standard deviation of the three repeated experiments.
[0018] Preparation Example 1 The antibacterial agent is prepared by the following method: (1) adding citric acid and hydroquinone to a 0.01M silver nitrate solution, controlling the stirring speed to 300 r / min, stirring for 40 minutes until uniform, heating to 60°C, and keeping the temperature and stirring for 40 minutes to obtain a silver solution; wherein the mass ratio of the silver nitrate solution, citric acid and hydroquinone is 12:1:1; (2) Chitosan powder was added to deionized water to obtain a chitosan solution with a mass concentration of 11%, and geraniol and silver solution were added in sequence while stirring. After stirring evenly, the pH was adjusted to 6.0. After standing for 3 hours, the antibacterial agent was obtained by filtering and drying, wherein the mass ratio of the chitosan solution, geraniol and silver solution was 30:1:8.
[0019] Preparation Example 2 The antibacterial agent is prepared by the following method: (1) Add citric acid and hydroquinone to a 0.05M silver nitrate solution, control the stirring speed to 400 r / min, stir for 30 minutes until uniform, then heat to 70°C, keep stirring for 30 minutes, and obtain a silver solution; wherein the mass ratio of the silver nitrate solution, citric acid and hydroquinone is 14:2:1; (2) Chitosan powder was added to deionized water to obtain a chitosan solution with a mass concentration of 13%, and geraniol and silver solution were added in sequence while stirring. After stirring evenly, the pH was adjusted to 6.5. After standing for 4 hours, the antibacterial agent was obtained by filtering and drying, wherein the mass ratio of the chitosan solution, geraniol and silver solution was 31:2:9.
[0020] Preparation Example 3 The antibacterial agent is prepared by the following method: (1) Add citric acid and hydroquinone to a 0.1 M silver nitrate solution, control the stirring speed to 500 r / min, stir for 20 minutes until uniform, then heat to 80°C, keep stirring for 20 minutes, and obtain a silver solution; wherein the mass ratio of the silver nitrate solution, citric acid and hydroquinone is 15:3:3; (2) Chitosan powder was added to deionized water to obtain a chitosan solution with a mass concentration of 15%, and geraniol and silver solution were added in sequence while stirring. After stirring evenly, the pH was adjusted to 7.0. After standing for 5 hours, the antibacterial agent was obtained by filtering and drying, wherein the mass ratio of the chitosan solution, geraniol and silver solution was 34:2:10.
[0021] Comparative Preparation Example 1 The antibacterial agent is prepared by the following method: (1) Add citric acid to a 0.01M silver nitrate solution, control the stirring speed to 300 r / min, stir for 40 minutes until uniform, then heat to 60°C, keep stirring for 40 minutes, and obtain a silver solution; wherein the mass ratio of the silver nitrate solution, citric acid and hydroquinone is 12:2; (2) Chitosan powder was added to deionized water to obtain a chitosan solution with a mass concentration of 11%, and geraniol and silver solution were added in sequence while stirring. After stirring evenly, the pH was adjusted to 6.0. After standing for 3 hours, the antibacterial agent was obtained by filtering and drying, wherein the mass ratio of the chitosan solution, geraniol and silver solution was 30:1:8.
[0022] Comparative Preparation Example 2 The antibacterial agent is prepared by the following method: (1) adding citric acid and hydroquinone to a 0.01M silver nitrate solution, controlling the stirring speed to 300 r / min, stirring for 40 minutes until uniform, heating to 60°C, and keeping the temperature and stirring for 40 minutes to obtain a silver solution; wherein the mass ratio of the silver nitrate solution, citric acid and hydroquinone is 12:1:1; (2) Chitosan powder was added to deionized water to obtain a chitosan solution with a mass concentration of 11%, and the silver solution was added in sequence while stirring. After stirring evenly, the pH was adjusted to 6.0. After standing for 3 hours, the antibacterial agent was obtained by filtering and drying, wherein the mass ratio of the chitosan solution to the silver solution was 30:8.
[0023] Example 1 A method for preparing a modified phenolic resin adhesive, specifically comprising the following preparation steps: S1: Add carbon fiber to acetic acid, soak at 60°C for 3h, wash repeatedly until neutral, and dry to obtain pretreated carbon fiber for standby use, wherein the mass ratio of carbon fiber to acetic acid is 1:8; disperse the pretreated carbon fiber in industrial ethanol, add a coupling agent, wherein the mass ratio of industrial ethanol, pretreated carbon fiber, and coupling agent is 100:28:4, and the coupling agent is composed of γ-aminopropyltrimethoxysilane and triisostearate titanate isopropyl ester in a mass ratio of 16:1, and stir the mixture evenly at room temperature until a stable carbon fiber dispersion is formed; 2-p-chlorobenzylpyridine, 1-butyl-3-methylimidazole chloride and fumaric acid are prepared into a mixed solvent according to a molar ratio of 8:1:1, and lignin, carbon fiber dispersion and ferric chloride are added thereto, wherein the mass ratio of the mixed solvent, lignin, carbon fiber dispersion and ferric chloride is 100:20:10:1, and stir continuously at 60°C for 6h, filter, wash and dry the mixture after uniform dispersion to obtain a functional filler.
[0024] S2: In parts by weight, 14 parts of phenol, 6 parts of functional fillers, 2 parts of melamine, 1 part of sodium hydroxide and 17 parts of 37% formaldehyde aqueous solution are added to 80 parts of tetrahydrofuran, and stirred at 80°C for 3 hours. Then, 17 parts of 37% formaldehyde aqueous solution are added to the reaction system, and stirring is continued at 80°C for 3 hours. After the reaction is completed, the modified phenolic resin is obtained by distillation under reduced pressure.
[0025] S3: By weight, 40 parts of modified phenolic resin, 16 parts of isopropyl alcohol, 1 part of dioctyl phthalate, 1 part of the antibacterial agent prepared in Preparation Example 1 and 80 parts of deionized water were weighed and mixed to obtain a modified phenolic resin adhesive.
[0026] Example 2 A method for preparing a modified phenolic resin adhesive, specifically comprising the following preparation steps: S1: Add carbon fiber to acetic acid, soak at 63°C for 2.8h, wash repeatedly until neutral, and dry to obtain pretreated carbon fiber for standby use, wherein the mass ratio of carbon fiber to acetic acid is 1:9; disperse the pretreated carbon fiber in industrial ethanol, add a coupling agent, wherein the mass ratio of industrial ethanol, pretreated carbon fiber, and coupling agent is 100:29:5, and the coupling agent is composed of γ-aminopropyltrimethoxysilane and triisostearate titanate isopropyl ester in a mass ratio of 17:1, and stir the above mixture evenly at room temperature until a stable carbon fiber dispersion is formed; 2-p-chlorobenzylpyridine, 1-butyl-3-methylimidazole chloride and fumaric acid are prepared into a mixed solvent according to a molar ratio of 9:2:1, and lignin, carbon fiber dispersion and ferric chloride are added thereto, wherein the mass ratio of the mixed solvent, lignin, carbon fiber dispersion and ferric chloride is 100:22:11:1, and stir continuously at 65°C for 5.5h, filter, wash and dry the mixture after the mixture is evenly dispersed to obtain a functional filler.
[0027] S2: By weight, 15 parts of phenol, 7 parts of functional fillers, 3 parts of melamine, 1.5 parts of sodium hydroxide and 18 parts of 37% formaldehyde aqueous solution are added to 80-100 parts of tetrahydrofuran, and stirred at 85°C for 2 hours. Then, 18 parts of 37% formaldehyde aqueous solution are added to the reaction system, and stirring is continued at 85°C for 2 hours. After the reaction is completed, the modified phenolic resin is obtained by distillation under reduced pressure.
[0028] S3: By weight, 42 parts of modified phenolic resin, 17 parts of isopropyl alcohol, 2 parts of dioctyl phthalate, 2 parts of the antibacterial agent prepared in Preparation Example 2 and 85 parts of deionized water were weighed and mixed to obtain a modified phenolic resin adhesive.
[0029] Example 3 A method for preparing a modified phenolic resin adhesive, specifically comprising the following preparation steps: S1: Add carbon fiber to acetic acid, soak at 65°C for 2.5 hours, wash repeatedly until neutral, and dry to obtain pretreated carbon fiber for standby use, wherein the mass ratio of carbon fiber to acetic acid is 1:9; disperse the pretreated carbon fiber in industrial ethanol, add a coupling agent, wherein the mass ratio of industrial ethanol, pretreated carbon fiber, and coupling agent is 100:30:6, and the coupling agent is composed of γ-aminopropyltrimethoxysilane and triisostearate titanate isopropyl ester in a mass ratio of 18:1, and stir the mixture evenly at room temperature until a stable carbon fiber dispersion is formed; 2-p-chlorobenzylpyridine, 1-butyl-3-methylimidazole chloride and fumaric acid are prepared into a mixed solvent according to a molar ratio of 10:2:2, and lignin, carbon fiber dispersion and ferric chloride are added thereto, wherein the mass ratio of the mixed solvent, lignin, carbon fiber dispersion and ferric chloride is 100:22:11:1, and stir continuously at 68°C for 5 hours, filter, wash and dry the mixture after uniform dispersion to obtain a functional filler.
[0030] S2: By weight, 16 parts of phenol, 8 parts of functional fillers, 4 parts of melamine, 2 parts of sodium hydroxide and 18 parts of 37% formaldehyde aqueous solution are added to 90 parts of tetrahydrofuran, and stirred at 85°C for 2 hours. Then, 17-19 parts of 37% formaldehyde aqueous solution are added to the reaction system, and stirring is continued at 85°C for 2 hours. After the reaction is completed, the modified phenolic resin is obtained by distillation under reduced pressure.
[0031] S3: By weight, 42 parts of modified phenolic resin, 18 parts of isopropyl alcohol, 2 parts of dioctyl phthalate, 2 parts of the antibacterial agent prepared in Preparation Example 2 and 90 parts of deionized water were weighed and mixed to obtain a modified phenolic resin adhesive.
[0032] Example 4 A method for preparing a modified phenolic resin adhesive, specifically comprising the following preparation steps: S1: Add carbon fiber to acetic acid, soak at 70°C for 2h, wash repeatedly until neutral, and dry to obtain pretreated carbon fiber for standby use, wherein the mass ratio of carbon fiber to acetic acid is 1:10; disperse the pretreated carbon fiber in industrial ethanol, add a coupling agent, wherein the mass ratio of industrial ethanol, pretreated carbon fiber, and coupling agent is 100:32:7, and the coupling agent is composed of γ-aminopropyltrimethoxysilane and triisostearate titanate isopropyl ester in a mass ratio of 20:1, and stir the above mixture evenly at room temperature until a stable carbon fiber dispersion is formed; 2-p-chlorobenzylpyridine, 1-butyl-3-methylimidazole chloride and fumaric acid are prepared into a mixed solvent according to a molar ratio of 12:3:3, and lignin, carbon fiber dispersion and ferric chloride are added thereto, wherein the mass ratio of the mixed solvent, lignin, carbon fiber dispersion and ferric chloride is 100:24:12:1, and stir continuously at 75°C for 4h, filter, wash and dry the mixture after uniform dispersion to obtain a functional filler.
[0033] S2: In parts by weight, 18 parts of phenol, 10 parts of functional fillers, 6 parts of melamine, 3 parts of sodium hydroxide and 19 parts of 37% formaldehyde aqueous solution are added to 100 parts of tetrahydrofuran, and after stirring at 90°C for 1 hour, 19 parts of 37% formaldehyde aqueous solution are added to the reaction system, and stirring is continued at 90°C for 1 hour. After the reaction is completed, the modified phenolic resin is obtained by distillation under reduced pressure.
[0034] S3: By weight, 44 parts of modified phenolic resin, 20 parts of isopropyl alcohol, 3 parts of dioctyl phthalate, 3 parts of the antibacterial agent prepared in Preparation Example 3 and 100 parts of deionized water were weighed and mixed to obtain a modified phenolic resin adhesive.
[0035] Comparative Example 1 A method for preparing a modified phenolic resin adhesive, specifically comprising the following preparation steps: S1: Add carbon fiber to acetic acid, soak at 60°C for 3h, wash repeatedly until neutral, and dry to obtain pretreated carbon fiber for use, wherein the mass ratio of carbon fiber to acetic acid is 1:8; disperse the pretreated carbon fiber in industrial ethanol, add γ-aminopropyltrimethoxysilane, wherein the mass ratio of industrial ethanol, pretreated carbon fiber, and γ-aminopropyltrimethoxysilane is 100:28:4, and stir the above mixture evenly at room temperature until a stable carbon fiber dispersion is formed; 2-p-chlorobenzylpyridine, 1-butyl-3-methylimidazole chloride and fumaric acid are prepared into a mixed solvent according to a molar ratio of 8:1:1, and lignin, carbon fiber dispersion and ferric chloride are added thereto, wherein the mass ratio of the mixed solvent, lignin, carbon fiber dispersion and ferric chloride is 100:20:10:1, and stir continuously at 60°C for 6h to make the mixture evenly dispersed, and then filter, wash and dry to obtain a functional filler.
[0036] S2: In parts by weight, 14 parts of phenol, 6 parts of functional fillers, 2 parts of melamine, 1 part of sodium hydroxide and 17 parts of 37% formaldehyde aqueous solution are added to 80 parts of tetrahydrofuran, and stirred at 80°C for 3 hours. Then, 17 parts of 37% formaldehyde aqueous solution are added to the reaction system, and stirring is continued at 80°C for 3 hours. After the reaction is completed, the modified phenolic resin is obtained by distillation under reduced pressure.
[0037] S3: By weight, 40 parts of modified phenolic resin, 16 parts of isopropyl alcohol, 1 part of dioctyl phthalate, 1 part of antibacterial agent and 80 parts of deionized water are weighed and mixed to obtain a modified phenolic resin adhesive.
[0038] Comparative Example 2 A method for preparing a modified phenolic resin adhesive, specifically comprising the following preparation steps: S1: Add carbon fiber to acetic acid, soak at 60°C for 3h, wash repeatedly until neutral, and dry to obtain pretreated carbon fiber for use, wherein the mass ratio of carbon fiber to acetic acid is 1:8; disperse the pretreated carbon fiber in industrial ethanol, add isopropyl titanate triisostearate, wherein the mass ratio of industrial ethanol, pretreated carbon fiber, and isopropyl titanate triisostearate is 100:28:4, and stir the mixture evenly at room temperature until a stable carbon fiber dispersion is formed; 2-p-chlorobenzylpyridine, 1-butyl-3-methylimidazole chloride and fumaric acid are prepared into a mixed solvent according to a molar ratio of 8:1:1, and lignin, carbon fiber dispersion and ferric chloride are added thereto, wherein the mass ratio of the mixed solvent, lignin, carbon fiber dispersion and ferric chloride is 100:20:10:1, and stir continuously at 60°C for 6h to filter, wash and dry the mixture after uniform dispersion to obtain a functional filler.
[0039] S2: In parts by weight, 14 parts of phenol, 6 parts of functional fillers, 2 parts of melamine, 1 part of sodium hydroxide and 17 parts of 37% formaldehyde aqueous solution are added to 80 parts of tetrahydrofuran, and stirred at 80°C for 3 hours. Then, 17 parts of 37% formaldehyde aqueous solution are added to the reaction system, and stirring is continued at 80°C for 3 hours. After the reaction is completed, the modified phenolic resin is obtained by distillation under reduced pressure.
[0040] S3: By weight, 40 parts of modified phenolic resin, 16 parts of isopropyl alcohol, 1 part of dioctyl phthalate, 1 part of antibacterial agent and 80 parts of deionized water are weighed and mixed to obtain a modified phenolic resin adhesive.
[0041] Comparative Example 3 A method for preparing a modified phenolic resin adhesive, specifically comprising the following preparation steps: S1: Add carbon fiber to acetic acid, soak at 60°C for 3h, wash repeatedly until neutral, and dry to obtain pretreated carbon fiber for standby use, wherein the mass ratio of carbon fiber to acetic acid is 1:8; disperse the pretreated carbon fiber in industrial ethanol, add a coupling agent, wherein the mass ratio of industrial ethanol, pretreated carbon fiber, and coupling agent is 100:28:4, and the coupling agent is composed of triisostearate isopropyl titanate and γ-aminopropyltrimethoxysilane in a mass ratio of 16:1. At room temperature, stir the mixture evenly until a stable carbon fiber dispersion is formed; prepare 2-p-chlorobenzylpyridine, 1-butyl-3-methylimidazole chloride and fumaric acid into a mixed solvent in a molar ratio of 8:1:1, add lignin, carbon fiber dispersion and ferric chloride thereto, wherein the mass ratio of the mixed solvent, lignin, carbon fiber dispersion and ferric chloride is 100:20:10:1, and stir continuously at 60°C for 6h to filter, wash and dry the mixture after uniform dispersion to obtain a functional filler.
[0042] S2: In parts by weight, 14 parts of phenol, 6 parts of functional fillers, 2 parts of melamine, 1 part of sodium hydroxide and 17 parts of 37% formaldehyde aqueous solution are added to 80 parts of tetrahydrofuran, and stirred at 80°C for 3 hours. Then, 17 parts of 37% formaldehyde aqueous solution are added to the reaction system, and stirring is continued at 80°C for 3 hours. After the reaction is completed, the modified phenolic resin is obtained by distillation under reduced pressure.
[0043] S3: By weight, 40 parts of modified phenolic resin, 16 parts of isopropyl alcohol, 1 part of dioctyl phthalate, 1 part of antibacterial agent and 80 parts of deionized water are weighed and mixed to obtain a modified phenolic resin adhesive.
[0044] Comparative Example 4 A method for preparing a modified phenolic resin adhesive, specifically comprising the following preparation steps: S1: Add carbon fiber to acetic acid, soak at 60°C for 3h, wash repeatedly until neutral, and dry to obtain pretreated carbon fiber for standby use, wherein the mass ratio of carbon fiber to acetic acid is 1:8; disperse the pretreated carbon fiber in industrial ethanol, add a coupling agent, wherein the mass ratio of industrial ethanol, pretreated carbon fiber, and coupling agent is 100:28:4, and the coupling agent is composed of γ-aminopropyltrimethoxysilane and triisostearate titanate isopropyl ester in a mass ratio of 16:1, and stir the mixture evenly at room temperature until a stable carbon fiber dispersion is formed; 2-p-chlorobenzylpyridine and 1-butyl-3-methylimidazole chloride are prepared into a solvent according to a molar ratio of 8:1, and lignin, carbon fiber dispersion and ferric chloride are added thereto, wherein the mass ratio of 1-butyl-3-methylimidazole chloride solvent, lignin, carbon fiber dispersion and ferric chloride is 100:20:10:1, and stir continuously at 60°C for 6h, filter, wash, and dry the mixture after uniform dispersion to obtain a functional filler.
[0045] S2: In parts by weight, 14 parts of phenol, 6 parts of functional fillers, 2 parts of melamine, 1 part of sodium hydroxide and 17 parts of 37% formaldehyde aqueous solution are added to 80 parts of tetrahydrofuran, and stirred at 80°C for 3 hours. Then, 17 parts of 37% formaldehyde aqueous solution are added to the reaction system, and stirring is continued at 80°C for 3 hours. After the reaction is completed, the modified phenolic resin is obtained by distillation under reduced pressure.
[0046] S3: By weight, 40 parts of modified phenolic resin, 16 parts of isopropyl alcohol, 1 part of dioctyl phthalate, 1 part of antibacterial agent and 80 parts of deionized water are weighed and mixed to obtain a modified phenolic resin adhesive.
[0047] Comparative Example 5 A method for preparing a modified phenolic resin adhesive, specifically comprising the following preparation steps: S1: Add carbon fiber to acetic acid, soak at 60°C for 3h, wash repeatedly until neutral, and dry to obtain pretreated carbon fiber for use, wherein the mass ratio of carbon fiber to acetic acid is 1:8; disperse the pretreated carbon fiber in industrial ethanol, add a coupling agent, wherein the mass ratio of industrial ethanol, pretreated carbon fiber, and coupling agent is 100:28:4, and the coupling agent is composed of γ-aminopropyltrimethoxysilane and triisostearate titanate isopropyl ester in a mass ratio of 16:1, and stir the mixture evenly at room temperature until a stable carbon fiber dispersion is formed; prepare 2-p-chlorobenzylpyridine and fumaric acid into a mixed solvent according to a molar ratio of 8:1, add lignin, carbon fiber dispersion and ferric chloride thereto, wherein the mass ratio of the mixed solvent, lignin, carbon fiber dispersion and ferric chloride is 100:20:10:1, and stir continuously at 60°C for 6h, filter, wash, and dry the mixture after uniform dispersion to obtain a functional filler.
[0048] S2: In parts by weight, 14 parts of phenol, 6 parts of functional fillers, 2 parts of melamine, 1 part of sodium hydroxide and 17 parts of 37% formaldehyde aqueous solution are added to 80 parts of tetrahydrofuran, and stirred at 80°C for 3 hours. Then, 17 parts of 37% formaldehyde aqueous solution are added to the reaction system, and stirring is continued at 80°C for 3 hours. After the reaction is completed, the modified phenolic resin is obtained by distillation under reduced pressure.
[0049] S3: By weight, 40 parts of modified phenolic resin, 16 parts of isopropyl alcohol, 1 part of dioctyl phthalate, 1 part of antibacterial agent and 80 parts of deionized water are weighed and mixed to obtain a modified phenolic resin adhesive.
[0050] Comparative Example 6 A method for preparing a modified phenolic resin adhesive, specifically comprising the following preparation steps: S1: Add carbon fiber to acetic acid, soak at 60°C for 3h, wash repeatedly until neutral, and dry to obtain pretreated carbon fiber for use, wherein the mass ratio of carbon fiber to acetic acid is 1:8; disperse the pretreated carbon fiber in industrial ethanol, add a coupling agent, wherein the mass ratio of industrial ethanol, pretreated carbon fiber, and coupling agent is 100:28:4, and the coupling agent is composed of γ-aminopropyltrimethoxysilane and triisostearate titanate isopropyl ester in a mass ratio of 16:1, and stir the mixture evenly at room temperature until a stable carbon fiber dispersion is formed; add lignin, carbon fiber dispersion and ferric chloride to N,N-dimethylformamide, wherein the mass ratio of N,N-dimethylformamide, lignin, carbon fiber dispersion and ferric chloride is 100:20:10:1, and stir continuously at 60°C for 6h, filter, wash, and dry the mixture after evenly dispersing it to obtain a functional filler.
[0051] S2: In parts by weight, 14 parts of phenol, 6 parts of functional fillers, 2 parts of melamine, 1 part of sodium hydroxide and 17 parts of 37% formaldehyde aqueous solution are added to 80 parts of tetrahydrofuran, and stirred at 80°C for 3 hours. Then, 17 parts of 37% formaldehyde aqueous solution are added to the reaction system, and stirring is continued at 80°C for 3 hours. After the reaction is completed, the modified phenolic resin is obtained by distillation under reduced pressure.
[0052] S3: By weight, 40 parts of modified phenolic resin, 16 parts of isopropyl alcohol, 1 part of dioctyl phthalate, 1 part of antibacterial agent and 80 parts of deionized water are weighed and mixed to obtain a modified phenolic resin adhesive.
[0053] Comparative Example 7 A method for preparing a modified phenolic resin adhesive, specifically comprising the following preparation steps: S1: Add carbon fiber to acetic acid, soak at 60°C for 3h, wash repeatedly until neutral, and dry to obtain pretreated carbon fiber for standby use, wherein the mass ratio of carbon fiber to acetic acid is 1:8; disperse the pretreated carbon fiber in industrial ethanol, add a coupling agent, wherein the mass ratio of industrial ethanol, pretreated carbon fiber, and coupling agent is 100:28:4, and the coupling agent is composed of γ-aminopropyltrimethoxysilane and triisostearate titanate isopropyl ester in a mass ratio of 16:1, and stir the mixture evenly at room temperature until a stable carbon fiber dispersion is formed; 2-p-chlorobenzylpyridine, 1-butyl-3-methylimidazole chloride and fumaric acid are prepared into a mixed solvent according to a molar ratio of 8:1:1, and lignin, carbon fiber dispersion and ferric chloride are added thereto, wherein the mass ratio of the mixed solvent, lignin, carbon fiber dispersion and ferric chloride is 100:20:10:1, and stir continuously at 60°C for 6h, filter, wash and dry the mixture after uniform dispersion to obtain a functional filler.
[0054] S2: By weight, 14 parts of phenol, 6 parts of functional fillers, 2 parts of melamine, 1 part of sodium hydroxide and 34 parts of 37% formaldehyde aqueous solution were added to 80 parts of tetrahydrofuran, and the mixture was stirred at 80°C for 6 hours. After the reaction was completed, the modified phenolic resin was obtained by vacuum distillation.
[0055] S3: By weight, 40 parts of modified phenolic resin, 16 parts of isopropyl alcohol, 1 part of dioctyl phthalate, 1 part of antibacterial agent and 80 parts of deionized water are weighed and mixed to obtain a modified phenolic resin adhesive.
[0056] Comparative Example 8 A method for preparing a modified phenolic resin adhesive, specifically comprising the following preparation steps: S1: Add carbon fiber to acetic acid, soak at 60°C for 3h, wash repeatedly until neutral, and dry to obtain pretreated carbon fiber for use, wherein the mass ratio of carbon fiber to acetic acid is 1:8; disperse the pretreated carbon fiber in industrial ethanol, add a coupling agent, wherein the mass ratio of industrial ethanol, pretreated carbon fiber, and coupling agent is 100:28:4, and the coupling agent is composed of γ-aminopropyltrimethoxysilane and triisostearate titanate isopropyl ester in a mass ratio of 16:1, and stir the mixture evenly at room temperature until a stable carbon fiber dispersion is formed; 2-p-chlorobenzylpyridine, 1-butyl-3-methylimidazole chloride and fumaric acid are prepared into a mixed solvent according to a molar ratio of 8:1:1, and lignin and carbon fiber dispersion are added thereto, wherein the mass ratio of the mixed solvent, lignin and carbon fiber dispersion is 100:20:10, and stir continuously at 60°C for 6h, filter, wash, and dry the mixture after uniform dispersion to obtain a functional filler.
[0057] S2: In parts by weight, 14 parts of phenol, 6 parts of functional fillers, 2 parts of melamine, 1 part of sodium hydroxide and 17 parts of 37% formaldehyde aqueous solution are added to 80 parts of tetrahydrofuran, and stirred at 80°C for 3 hours. Then, 17 parts of 37% formaldehyde aqueous solution are added to the reaction system, and stirring is continued at 80°C for 3 hours. After the reaction is completed, the modified phenolic resin is obtained by distillation under reduced pressure.
[0058] S3: By weight, 40 parts of modified phenolic resin, 16 parts of isopropyl alcohol, 1 part of dioctyl phthalate, 1 part of antibacterial agent and 80 parts of deionized water are weighed and mixed to obtain a modified phenolic resin adhesive.
[0059] Comparative Example 9 A method for preparing a modified phenolic resin adhesive, specifically comprising the following preparation steps: S1: Add carbon fiber to acetic acid, soak at 60°C for 3h, wash repeatedly until neutral, and dry to obtain pretreated carbon fiber for standby use, wherein the mass ratio of carbon fiber to acetic acid is 1:8; disperse the pretreated carbon fiber in industrial ethanol, add a coupling agent, wherein the mass ratio of industrial ethanol, pretreated carbon fiber, and coupling agent is 100:28:4, and the coupling agent is composed of γ-aminopropyltrimethoxysilane and triisostearate titanate isopropyl ester in a mass ratio of 16:1, and stir the mixture evenly at room temperature until a stable carbon fiber dispersion is formed; 2-p-chlorobenzylpyridine, 1-butyl-3-methylimidazole chloride and fumaric acid are prepared into a mixed solvent according to a molar ratio of 8:1:1, and lignin, carbon fiber dispersion and ferric chloride are added thereto, wherein the mass ratio of the mixed solvent, lignin, carbon fiber dispersion and ferric chloride is 100:20:10:1, and stir continuously at 60°C for 6h, filter, wash and dry the mixture after uniform dispersion to obtain a functional filler.
[0060] S2: In parts by weight, 14 parts of phenol, 6 parts of functional fillers, 2 parts of melamine, 1 part of sodium hydroxide and 17 parts of 37% formaldehyde aqueous solution are added to 80 parts of tetrahydrofuran, and stirred at 80°C for 3 hours. Then, 17 parts of 37% formaldehyde aqueous solution are added to the reaction system, and stirring is continued at 80°C for 3 hours. After the reaction is completed, the modified phenolic resin is obtained by distillation under reduced pressure.
[0061] S3: By weight, 40 parts of modified phenolic resin, 16 parts of isopropyl alcohol, 1 part of dioctyl phthalate, 1 part of the antibacterial agent prepared in Comparative Preparation Example 1 and 80 parts of deionized water were weighed and mixed to obtain a modified phenolic resin adhesive.
[0062] Comparative Example 10 A method for preparing a modified phenolic resin adhesive, specifically comprising the following preparation steps: S1: Add carbon fiber to acetic acid, soak at 60°C for 3h, wash repeatedly until neutral, and dry to obtain pretreated carbon fiber for standby use, wherein the mass ratio of carbon fiber to acetic acid is 1:8; disperse the pretreated carbon fiber in industrial ethanol, add a coupling agent, wherein the mass ratio of industrial ethanol, pretreated carbon fiber, and coupling agent is 100:28:4, and the coupling agent is composed of γ-aminopropyltrimethoxysilane and triisostearate titanate isopropyl ester in a mass ratio of 16:1, and stir the mixture evenly at room temperature until a stable carbon fiber dispersion is formed; 2-p-chlorobenzylpyridine, 1-butyl-3-methylimidazole chloride and fumaric acid are prepared into a mixed solvent according to a molar ratio of 8:1:1, and lignin, carbon fiber dispersion and ferric chloride are added thereto, wherein the mass ratio of the mixed solvent, lignin, carbon fiber dispersion and ferric chloride is 100:20:10:1, and stir continuously at 60°C for 6h, filter, wash and dry the mixture after uniform dispersion to obtain a functional filler.
[0063] S2: In parts by weight, 14 parts of phenol, 6 parts of functional fillers, 2 parts of melamine, 1 part of sodium hydroxide and 17 parts of 37% formaldehyde aqueous solution are added to 80 parts of tetrahydrofuran, and stirred at 80°C for 3 hours. Then, 17 parts of 37% formaldehyde aqueous solution are added to the reaction system, and stirring is continued at 80°C for 3 hours. After the reaction is completed, the modified phenolic resin is obtained by distillation under reduced pressure.
[0064] S3: By weight, 40 parts of modified phenolic resin, 16 parts of isopropyl alcohol, 1 part of dioctyl phthalate, 1 part of the antibacterial agent prepared in Comparative Preparation Example 2 and 80 parts of deionized water were weighed and mixed to obtain a modified phenolic resin adhesive.
[0065] Performance Testing The following performance tests were carried out on a modified phenolic resin adhesive prepared in the above experiment: 1. Formaldehyde Residue The formaldehyde residue in the phenolic resin adhesive prepared in each embodiment and comparative example was tested according to GB / T 32461-2015 "Determination of formaldehyde content in amino resins and phenolic resins and formaldehyde migration in their molded products by high performance liquid chromatography". The test results are shown in Table 1.
[0066] The residual phenol content in the phenolic resin adhesives prepared in the examples and comparative examples was tested according to the method provided in HG / T 2621-1994 "Determination of residual phenol content in phenolic resin by gas chromatography".
[0067] Mechanical properties bonding strength test: Adhesive is applied to the wood board in the coating method specified in the national standard GB / T 17657-2013, and then processed, and finally tested in the tensile shearing machine mode; According to GB / T 9846-2015 "Ordinary plywood" impact strength of adhesive coated boards The test results are shown in Table 1.
[0068] The antibacterial performance was tested according to the requirements and steps of the national standard GB / T 31402-2015 Plastic Surface Antibacterial Performance Test Method, and the test bacteria were Staphylococcus aureus and Escherichia coli. The antibacterial persistence test method was based on the national standard GB / T31402-2015. After the sample was placed for 90 days, the antibacterial rate was tested. The test results are shown in Table 2.
[0069] Table 1 Comprehensive properties of adhesives prepared in Examples 1-4 and Comparative Examples 1-10
[0070] Table 2 Antibacterial properties of adhesives prepared in Examples 1-4 and Comparative Examples 9-10
[0071] From the results shown in Table 1 and Table 2 above, it can be seen that the comprehensive performance of the modified phenolic resin adhesives prepared in Examples 1-4 of the present invention is much better than that of Comparative Examples 1-10.
[0072] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. A method for preparing a modified phenolic resin adhesive, characterized in that: The method comprises the following preparation steps: S1. Dispersing the carbon fiber treated with organic acid in industrial ethanol, adding a coupling agent thereto, and stirring evenly at room temperature to obtain a carbon fiber dispersion; adding lignin, the carbon fiber dispersion and Lewis acid to the mixed solvent, stirring continuously at 60-75° C. for 4-6 hours to uniformly disperse the mixture, filtering, washing and drying to obtain a functional filler; S2, dissolving phenol in tetrahydrofuran, adding melamine, sodium hydroxide and functional filler to phenol-tetrahydrofuran, stirring continuously at 80-90° C. for 1-3 h, adding the first batch of 37% formaldehyde aqueous solution, stirring continuously at 80-90° C. for 1-3 h, adding the second batch of 37% formaldehyde aqueous solution, and distilling under reduced pressure after completion of the reaction to obtain a modified phenolic resin; S3, mixing the modified phenolic resin, the antibacterial agent, the diluent, the plasticizer and the deionized water to obtain a modified phenolic resin adhesive.
2. The method for preparing the modified phenolic resin adhesive according to claim 1, characterized in that: The coupling agent in step S1 is composed of γ-aminopropyltrimethoxysilane and isopropyl titanate triisostearate in a mass ratio of 16-20:
1.
3. The method for preparing the modified phenolic resin adhesive according to claim 1, characterized in that: The mixed solvent in step S1 is composed of 2-p-chlorobenzylpyridine, 1-butyl-3-methylimidazole chloride and fumaric acid in a molar ratio of 8-12:1-3:1-3.
4. The method for preparing the modified phenolic resin adhesive according to claim 1, characterized in that: The Lewis acid in step S1 is any one of ferric chloride, aluminum chloride and aluminum oxide.
5. The method for preparing the modified phenolic resin adhesive according to claim 1, characterized in that: In step S2, the components by weight include 14-18 parts of phenol, 6-10 parts of functional fillers, 2-6 parts of melamine, 1-3 parts of sodium hydroxide, 34-38 parts of 37% formaldehyde aqueous solution and 80-100 parts of tetrahydrofuran.
6. The method for preparing the modified phenolic resin adhesive according to claim 1, characterized in that: In step S3, the components by weight include 40-44 parts of modified phenolic resin, 16-20 parts of diluent, 1-3 parts of plasticizer, 1-3 parts of antibacterial agent and 80-100 parts of deionized water.
7. The method for preparing the modified phenolic resin adhesive according to claim 1, characterized in that: The diluent in step S3 is at least one of isopropanol, ethanol and ethylene glycol.
8. The method for preparing the modified phenolic resin adhesive according to claim 1, characterized in that: The antibacterial agent in step S3 is prepared by the following method: (1) Add citric acid and hydroquinone to a 0.01-0.1 M silver nitrate solution, stir evenly, heat to 60-80°C, and stir for 20-40 minutes to obtain a silver solution; (2) Add chitosan powder to deionized water to prepare a chitosan solution with a mass concentration of 11-15%, add geraniol and silver solution in sequence while stirring, adjust the pH to 6.0-7.0 after stirring evenly, let it stand for 3-5 hours, filter and dry to obtain the antibacterial agent.
9. The method for preparing the modified phenolic resin adhesive according to claim 1, characterized in that: The plasticizer in step S3 is at least one of dioctyl phthalate, triphenyl phosphate, and dipentaerythritol ester.
10. A modified phenolic resin adhesive, characterized in that: The adhesive is prepared by the method for preparing the modified phenolic resin adhesive according to any one of claims 1 to 9.
Citation Information
Patent Citations
Preparation method of carbon fiber modified phenolic resin and phenolic moulding plastic
CN105754056A
Phenolic resin adhesive with low free formaldehyde content and preparation method thereof
CN116640543A