Boron trifluoride monoethylamine-based high-performance epoxy resin adhesive as well as preparation and use methods thereof

By using triarylsulfonium hexafluorate in epoxy resin adhesives to activate monomers and nanometals, the problems of poor mechanical properties of the adhesive and long initial curing time in the prior art are solved, and the complete curing and improvement of the adhesive are achieved Good adhesion, suitable for electronic and electrical appliance fields.

CN118931444AActive Publication Date: 2024-11-12ZHENGZHOU UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411013576.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-12
Estimated Expiration
2044-07-26

AI Technical Summary

Technical Problem

The existing epoxy resin adhesives have problems such as high thermal curing temperature, inconvenient two-component composition, long initial curing time and poor environmental protection in the field of electronic and electrical appliances, and low molecular oxygen-containing cyclic by-products in boron trifluoride monoethylamine system. Generate influencing mechanical properties.

Method used

Protic acid is generated by adding triarylsulfonium hexafluoroantionicate or triarylsulfonium hexafluorophosphate, and the activation monomer works synergistically with boron trifluoride monoethylamine, combines nanometals, and regulates the ratio to inhibit the generation of by-products. and shorten the initial curing time and optimize the mechanical properties and adhesion of the adhesive.

Benefits of technology

It significantly improves the mechanical properties of the adhesive, shortens the initial curing time, avoids slippage, achieves complete curing of the adhesive and better metal surface adhesion, and improves application efficiency and mechanical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004965075190000061
    Figure BDA0004965075190000061
Patent Text Reader

Abstract

The invention discloses a high-performance epoxy resin adhesive based on boron trifluoride monoethylamine as well as preparation and use methods thereof, specific triaryl sulfonium hexafluoride is added into a boron trifluoride monoethylamine epoxy resin system, protonic acid is generated and acts on an epoxy group to generate an activated monomer, and the high-performance epoxy resin adhesive based on boron trifluoride monoethylamine is prepared. The activated monomer and the boron trifluoride monoethylamine have a synergistic effect, so that the generation of low-molecular oxygen-containing cyclic by-products in a boron trifluoride monoethylamine epoxy resin system can be effectively avoided, the problem of poor mechanical properties of the existing boron trifluoride monoethylamine-based epoxy resin adhesive is solved, and meanwhile, due to the action of light, the mechanical properties of the epoxy resin adhesive are improved. The initial curing time of the adhesive is remarkably shortened, slippage of the adhesive is effectively avoided, and pre-bonding is achieved. The nano-metal is added, so that the cohesive energy of a system is reduced, and the cohesive property of the epoxy resin adhesive and the metal surface is enhanced; besides, by optimizing and screening a formula and regulating and controlling the part ratio of the triaryl sulfonium hexafluoride to the boron trifluoride monoethylamine in a specific range, the generation of low-molecular cyclic epoxy by-products of a system can be inhibited to the greatest extent, and meanwhile, the complete curing of the epoxy resin adhesive can be realized, so that the epoxy resin adhesive achieves the optimal mechanical property.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of epoxy resin adhesives, and specifically relates to a high-performance epoxy resin adhesive based on boron trifluoride monoethylamine and a preparation method and a use method thereof. Background Art

[0002] Epoxy resin adhesive is a kind of engineering adhesive made of epoxy resin base material, curing agent, diluent, accelerator, filler, etc. Due to its good bonding performance, good functionality, low price and simple bonding process, it has been widely used in the fields of home appliances, automobiles, water conservancy and transportation, electronic appliances and aerospace industry in recent decades.

[0003] The epoxy resin adhesives currently used in the field of electronic appliances have the following problems: 1. The thermal curing temperature is high, which can easily damage precision electronic devices; 2. It is composed of two components and cannot be mixed in advance, which is inconvenient to use; 3. The initial curing time is long, it is easy to slip, and affects the efficiency; 4. It is environmentally friendly and uses organic solvents such as acetone and N,N-dimethylformamide during the preparation process.

[0004] Boron trifluoride monoethylamine is a latent curing agent for epoxy resin, which has the advantages of low-temperature curing and latent characteristics. It can not only machine various immersion parts before curing, but also the reaction system formed by it and epoxy resin does not require any solvent, is green and environmentally friendly, has a single component composition, and is easy to operate. Therefore, the epoxy resin adhesive based on boron trifluoride monoethylamine can solve most of the problems of epoxy adhesives in the prior art, but the system also has certain problems. During the reaction process of the boron trifluoride monoethylamine epoxy resin adhesive system, low molecular oxygen-containing cyclic byproducts will be generated, and the curing is incomplete, thereby affecting the mechanical properties of the adhesive. At present, hydroxyl-containing compounds are generally added to inhibit the generation of the byproducts, but this method has the following problems: 1. The mechanical properties are poor. Excessive addition of hydroxyl compounds inhibits the generation of byproducts and also reduces the relative addition content of epoxy resin, resulting in reduced mechanical properties of the adhesive; 2. The initial curing time is long, which easily leads to slippage of the adhesive, affecting efficiency and reducing mechanical properties. Therefore, there is an urgent need for a high-performance epoxy resin adhesive based on boron trifluoride monoethylamine that can solve the above technical problems. Summary of the invention

[0005] Based on the deficiencies of the prior art, the present invention provides a high-performance epoxy resin adhesive based on boron trifluoride monoethylamine and a preparation and use method thereof. By adding triarylsulfonium hexafluoroantimonate or triarylsulfonium hexafluorophosphate (referred to as specific triarylsulfonium hexafluorophosphate), protonic acid is generated by the triarylsulfonium hexafluorophosphate and acts on epoxy groups to generate activated monomers. The activated monomers and boron trifluoride monoethylamine act synergistically to effectively avoid the generation of low-molecular oxygen-containing cyclic by-products, thereby solving the problem of poor mechanical properties of the existing epoxy resin adhesive based on boron trifluoride monoethylamine. At the same time, due to the effect of light, the initial curing time of the adhesive is significantly shortened, effectively avoiding the slippage of the adhesive and achieving pre-bonding. The invention reduces the cohesive energy of the system and enhances the adhesion between the epoxy resin adhesive and the metal surface by adding nano-metal; in addition, the invention adjusts the proportion of a specific triarylsulfonium hexafluoride and boron trifluoride monoethylamine within a specific range through formula optimization and screening, which can not only inhibit the generation of by-products to the greatest extent but also realize the complete curing of the adhesive, so that the boron trifluoride monoethylamine epoxy resin adhesive achieves the best mechanical properties.

[0006] The present invention provides a high-performance epoxy resin adhesive based on boron trifluoride monoethylamine, the raw material composition and weight proportion of which are as follows:

[0007] 80-95 parts of epoxy resin 4,5-epoxycyclohexane-1,2-dicarboxylic acid diglycidyl ester;

[0008] Thermal curing agent boron trifluoride monoethylamine 2.0-8.0 parts;

[0009] Photoinitiator 2.0-12.0 parts;

[0010] Nano metal 0.1-10 parts;

[0011] The photoinitiator is one of triarylsulfonium hexafluoroantimonate and triarylsulfonium hexafluorophosphate;

[0012] The ratio of the raw materials should meet the following conditions:

[0013] The ratio of the photoinitiator triarylsulfonium hexafluoride to the thermal curing agent boron trifluoride monoethylamine is between 1.0 and 1.5;

[0014] The nano metal is one or more combinations of nano iron powder, nano copper powder and nano aluminum powder.

[0015] The nano metal particle size is between 30-200 nm.

[0016] Furthermore, the method for preparing a high-performance epoxy resin adhesive based on boron trifluoride monoethylamine comprises the following steps:

[0017] (1) Weigh each raw material according to weight;

[0018] (2) adding weighed epoxy resin 4,5-epoxycyclohexane-1,2-dicarboxylic acid diglycidyl ester and thermal curing agent boron trifluoride monoethylamine at water bath temperature, and stirring magnetically to obtain system 1;

[0019] (3) adding a photoinitiator triarylsulfonium hexafluoride to the resin system 1 obtained in step (2), stirring the mixture evenly with a magnetic stirrer in a dark environment, then adding the nano-metal and continuing to stir the mixture evenly with a magnetic stirrer in a dark environment, and placing the mixture in an ultrasonic bath to disperse the mixture evenly to obtain a system 2;

[0020] (4) degassing the system 2 obtained in step (3) under vacuum conditions and cooling to room temperature to obtain a high-performance epoxy resin adhesive.

[0021] The water bath temperature in step (2) is 40-70°C.

[0022] In the step (3), the magnetic stirring time is 20 to 90 minutes, and the stirring rate is 300 to 600 r / min.

[0023] In the step (3), the ultrasonic power is 1000-1800 W, and the ultrasonic time is 5-30 min.

[0024] The vacuum degassing time in step (4) is 5 to 30 minutes.

[0025] Furthermore, the method for using the high-performance epoxy resin adhesive based on boron trifluoride monoethylamine includes using the adhesive after light or heat curing.

[0026] The conditions of the photothermal curing include: light wavelength 315-400nm, irradiation time 1-2min, temperature 80-120°C, time 2-6h.

[0027] Compared with the prior art, the present invention has the following beneficial effects:

[0028] (1) The present invention adds a specific triarylsulfonium hexafluoride to the boron trifluoride monoethylamine epoxy resin adhesive system, utilizes the triarylsulfonium hexafluoride to generate proton acid, and acts on the epoxy group to generate an activated monomer. The activated monomer and the boron trifluoride monoethylamine act synergistically, and the generation of low molecular weight oxygen-containing cyclic byproducts in the boron trifluoride monoethylamine epoxy resin system can be effectively avoided, thereby solving the problem of poor mechanical properties of the existing boron trifluoride monoethylamine-based epoxy resin adhesive. At the same time, due to the effect of light, the initial curing time of the adhesive is significantly shortened, effectively avoiding the slippage of the adhesive, and achieving pre-bonding.

[0029] (2) The present invention optimizes and screens the formula to adjust the ratio of triarylsulfonium hexafluoride to boron trifluoride monoethylamine to between 1.0 and 1.5, which can avoid the generation of by-products to the greatest extent and also achieve complete curing of the epoxy resin adhesive. When the ratio of triarylsulfonium hexafluoride to boron trifluoride monoethylamine is low, that is, the amount of boron trifluoride monoethylamine is relatively large, the proton acid generated by triarylsulfonium hexafluoride is not enough to completely inhibit the generation of low molecular oxygen-containing cyclic by-products in the boron trifluoride monoethylamine epoxy resin system, affecting the mechanical properties of the adhesive; when the ratio of the two is high, that is, the amount of boron trifluoride monoethylamine is small, the cross-linking depth of the adhesive curing network is insufficient, and it cannot be completely cured, which can also lead to a decrease in the mechanical properties of the adhesive. Therefore, when the ratio of the two is controlled within a specific range between 1.0 and 1.5, the best mechanical properties can be achieved.

[0030] (3) The present invention reduces the cohesive energy of the system by adding nano-metal, enhances the interaction between the epoxy resin adhesive and the metal surface, promotes better adhesion of the adhesive to the metal material, and significantly improves the mechanical properties. DETAILED DESCRIPTION

[0031] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with embodiments and comparative examples.

[0032] In the following examples and comparative examples, 4,5-epoxycyclohexane-1,2-dicarboxylic acid diglycidyl ester epoxy resin was purchased from Tianjin Jingdong Chemical Composite Materials Co., Ltd., boron trifluoride monoethylamine was purchased from Shanghai Aladdin Biochemical Technology Co., Ltd., triarylsulfonium hexafluoride was purchased from Wuhan Huaxiang Keqi Biotechnology Co., Ltd., and nanometals were purchased from Shanghai Guangyi Chemical Co., Ltd.

[0033] Example 1

[0034] A high-performance epoxy resin adhesive based on boron trifluoride monoethylamine is prepared from the following raw materials in parts by weight: 86 parts of 4,5-epoxycyclohexane-1,2-dicarboxylic acid diglycidyl ester, 6.0 parts of boron trifluoride monoethylamine as a thermal curing agent, 6.0 parts of triarylsulfonium hexafluoroantimonate as a photoinitiator, and 2.0 parts of nano iron powder.

[0035] The preparation method of the high-performance epoxy resin adhesive comprises the following steps:

[0036] (1) Weigh each raw material according to weight;

[0037] (2) adding weighed epoxy resin 4,5-epoxycyclohexane-1,2-dicarboxylic acid diglycidyl ester and thermal curing agent boron trifluoride monoethylamine at a water bath temperature of 55° C. and stirring at a magnetic force of 400 r / min for 40 min to obtain system 1;

[0038] (3) adding triarylsulfonium hexafluoroantimonate to the resin system 1 obtained in step (2), stirring at 400 r / min under a dark condition for 50 min, then adding nano iron powder and continuing to stir, placing in a 1500 W ultrasonic bath for 15 min, and uniformly dispersing to obtain system 2;

[0039] (4) Degas the system 2 obtained in step (3) under vacuum conditions for 20 minutes and cool it to room temperature to obtain a high-performance epoxy resin adhesive.

[0040] The obtained epoxy resin adhesive was irradiated with 365 nm wavelength light for 1.5 min and placed in a 120°C oven for 4 h before mechanical property testing.

[0041] Example 2

[0042] A high-performance epoxy resin adhesive based on boron trifluoride monoethylamine is prepared from the following raw materials in parts by weight: 84.5 parts of 4,5-epoxycyclohexane-1,2-dicarboxylic acid diglycidyl ester, 6.0 parts of boron trifluoride monoethylamine as a thermal curing agent, 7.5 parts of triarylsulfonium hexafluoroantimonate as a photoinitiator, and 2.0 parts of nano iron powder.

[0043] The preparation method of the high-performance epoxy resin adhesive comprises the following steps:

[0044] (1) Weigh each raw material according to weight;

[0045] (2) adding weighed epoxy resin 4,5-epoxycyclohexane-1,2-dicarboxylic acid diglycidyl ester and thermal curing agent boron trifluoride monoethylamine at a water bath temperature of 55° C. and stirring at a magnetic force of 400 r / min for 40 min to obtain system 1;

[0046] (3) adding triarylsulfonium hexafluoroantimonate to the resin system 1 obtained in step (2), stirring the mixture at 400 r / min in a dark environment for 50 min, then adding nano iron powder and continuing to stir the mixture in a dark environment, ultrasonically treating the mixture at 1500 W for 15 min to uniformly disperse the mixture, and obtaining system 2;

[0047] (4) Degas the system 2 obtained in step (3) under vacuum conditions for 20 minutes and cool it to room temperature to obtain a high-performance epoxy resin adhesive.

[0048] The obtained epoxy resin adhesive was irradiated with 365 nm wavelength light for 1.5 min and placed in a 120°C oven for 4 h before mechanical property testing.

[0049] Example 3

[0050] A high-performance epoxy resin adhesive based on boron trifluoride monoethylamine is prepared from the following raw materials in parts by weight: 83 parts of 4,5-epoxycyclohexane-1,2-dicarboxylic acid diglycidyl ester, 6.0 parts of boron trifluoride monoethylamine as a thermal curing agent, 9.0 parts of triarylsulfonium hexafluoroantimonate as a photoinitiator, and 2.0 parts of nano iron powder.

[0051] The preparation method of the high-performance epoxy resin adhesive comprises the following steps:

[0052] (1) Weigh each raw material according to weight;

[0053] (2) adding weighed epoxy resin 4,5-epoxycyclohexane-1,2-dicarboxylic acid diglycidyl ester and thermal curing agent boron trifluoride monoethylamine at a water bath temperature of 55° C. and stirring at a magnetic force of 400 r / min for 40 min to obtain system 1;

[0054] (3) adding triarylsulfonium hexafluoroantimonate to the resin system 1 obtained in step (2), stirring the mixture at 400 r / min in a dark environment for 50 min, then adding nano iron powder and continuing to stir the mixture in a dark environment, ultrasonically treating the mixture at 1500 W for 15 min to uniformly disperse the mixture, and obtaining system 2;

[0055] (4) Degas the system 2 obtained in step (3) under vacuum conditions for 20 minutes and cool it to room temperature to obtain a high-performance epoxy resin adhesive.

[0056] The obtained epoxy resin adhesive was irradiated with 365 nm wavelength light for 1.5 min and placed in a 120°C oven for 4 h before mechanical property testing.

[0057] Comparative Example 1

[0058] A conventional boron trifluoride monoethylamine epoxy resin adhesive is prepared from the following raw materials in parts by weight: 84.5 parts of 4,5-epoxycyclohexane-1,2-dicarboxylic acid diglycidyl ester, 6.0 parts of a thermal curing agent boron trifluoride monoethylamine, 7.5 parts of a polyhydroxy compound (propylene glycol), and 2.0 parts of nano iron powder.

[0059] The preparation method of the high-performance epoxy resin adhesive comprises the following steps:

[0060] (1) Weigh each raw material according to weight;

[0061] (2) adding weighed epoxy resin 4,5-epoxycyclohexane-1,2-dicarboxylic acid diglycidyl ester and thermal curing agent boron trifluoride monoethylamine at a water bath temperature of 55° C. and stirring at a magnetic force of 400 r / min for 40 min to obtain system 1;

[0062] (3) Adding a polyhydroxy compound (propylene glycol) to the resin system 1 obtained in step (2), stirring the mixture at 400 r / min under light-proof conditions for 50 min, then adding nano iron powder and continuing to stir the mixture under light-proof conditions, placing the mixture in a 1500 W ultrasonic bath for 15 min to uniformly disperse the mixture, and obtaining a system 2;

[0063] (4) degassing the system 2 obtained in step (3) under vacuum conditions for 20 minutes and cooling to room temperature to obtain a conventional boron trifluoride monoethylamine epoxy resin adhesive.

[0064] The obtained conventional epoxy resin adhesive was placed in an oven at 120°C for 4 h and then the mechanical properties test was performed.

[0065] The shear strength test of the corresponding products of the above-mentioned Examples 1-3 and Comparative Example 1 was tested on a Sansi CMT universal tensile testing machine, and the test standard was based on GB / T 7124-2008; the initial solidification time was measured (the initial solidification time refers to the time from the liquid mixture to the initial reaction to become a solid), and the timer was used for timing.

[0066] The results are as follows:

[0067] Table 1 Examples and Comparative Examples Results

[0068]

[0069] The above test results show that: 1. Compared with the traditional method of adding hydroxyl-containing chemical substances (Comparative Example 1), the mechanical shear strength of the high-performance epoxy resin adhesive based on boron trifluoride monoethylamine prepared by the present invention (Examples 1-3) is greatly improved, and the maximum can reach 25.3MPa, which is 2.18 times that of the comparative example; 2. The initial curing time of Examples 1-3 of the present invention is 1.5min, while the initial curing time of Comparative Example 1 is 90min. This experimental result shows that the adhesive of the present invention significantly shortens the initial curing time through the action of light, effectively avoids the slippage of the adhesive, and realizes pre-bonding; 3. The ratio of triarylsulfonium hexafluoride to boron trifluoride monoethylamine in Examples 1-3 is 1.00, 1.25, and 1.50 respectively. When the ratio of the two reaches 1. 25, it has the highest shear strength, which is 25.3MPa. This is mainly because at this ratio, it can not only inhibit the low molecular oxygen-containing cyclic by-products produced in the boron trifluoride monoethylamine epoxy resin adhesive system to the greatest extent, but also enable the adhesive to be completely cured, and the synergistic effect of the two reaches the best; 4. When the ratio of triarylsulfonium hexafluoride to boron trifluoride monoethylamine is low, that is, the proportion of boron trifluoride monoethylamine is relatively large, the proton acid produced by triarylsulfonium hexafluoride is not enough to completely inhibit the formation of low molecular oxygen-containing cyclic by-products in the boron trifluoride monoethylamine epoxy resin system, affecting the mechanical properties of the adhesive; when the ratio of the two is high, that is, the proportion of boron trifluoride monoethylamine is small, the cross-linking depth of the adhesive curing network is insufficient, and it cannot be completely cured, which can also lead to a decrease in the mechanical properties of the adhesive.

[0070] In summary, the high-performance epoxy resin adhesive provided by the present invention solves the problems existing in the existing epoxy resin adhesive based on boron trifluoride monoethylamine, greatly improves the mechanical properties of the adhesive, and significantly shortens the initial curing time of the adhesive, solves the problem of adhesive slippage, and achieves pre-bonding, so that the adhesive system has good application prospects in the field of electronic appliances.

[0071] The above embodiments only express several implementation methods of the present invention, but they cannot be understood as limiting the scope of the patent of the present invention. It should be pointed out that for ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be based on the attached claims.

[0072] The above are merely embodiments and comparative examples of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A high performance epoxy resin adhesive based on boron trifluoride monoethylamine, characterized in that: The raw material composition and weight ratio are as follows: 80-95 parts of epoxy resin 4,5-epoxycyclohexane-1,2-dicarboxylic acid diglycidyl ester; Thermal curing agent boron trifluoride monoethylamine 2.0-8.0 parts; Photoinitiator 2.0-12.0 parts; Nano metal 0.1-10 parts; The photoinitiator is one of triarylsulfonium hexafluoroantimonate and triarylsulfonium hexafluorophosphate; The raw material ratio should meet the following conditions: The ratio of the photoinitiator to the thermal curing agent boron trifluoride monoethylamine in the component is controlled to be between 1.0 and 1.

5.

2. A high performance epoxy resin adhesive based on boron trifluoride monoethylamine according to claim 1, characterized in that: The nano metal is one or more combinations of nano iron powder, nano copper powder and nano aluminum powder.

3. The high-performance epoxy resin adhesive based on boron trifluoride monoethylamine according to claim 1, characterized in that: The nano metal particle size is between 30-200 nm.

4. The high-performance epoxy resin adhesive based on boron trifluoride monoethylamine according to claim 1, wherein the preparation method comprises the following steps: (1) Weigh each raw material according to weight; (2) adding weighed epoxy resin 4,5-epoxycyclohexane-1,2-dicarboxylic acid diglycidyl ester and thermal curing agent boron trifluoride monoethylamine at water bath temperature, and stirring magnetically to obtain system 1; (3) adding a photoinitiator triarylsulfonium hexafluoride to the system 1 obtained in step (2), stirring the mixture evenly under magnetic stirring in the dark, then adding the nanometal and continuing to stir the mixture evenly under magnetic stirring in the dark, placing the mixture in an ultrasonic bath, and dispersing the mixture evenly to obtain a system 2; (4) degassing the system 2 obtained in step (3) under vacuum conditions and cooling to room temperature to obtain a high-performance epoxy resin adhesive.

5. The method for preparing a high-performance epoxy resin adhesive based on boron trifluoride monoethylamine according to claim 4, characterized in that: The water bath temperature in step (2) is 40-70°C.

6. The method for preparing a high-performance epoxy resin adhesive based on boron trifluoride monoethylamine according to claim 4, characterized in that: In the step (3), the magnetic stirring time is 20 to 90 minutes, and the stirring rate is 300 to 600 r / min.

7. The method for preparing a high-performance epoxy resin adhesive based on boron trifluoride monoethylamine according to claim 4, characterized in that: In the step (3), the ultrasonic power is 1000-1800W, and the ultrasonic time is 5-30min.

8. The method for preparing a high-performance epoxy resin adhesive based on boron trifluoride monoethylamine according to claim 4, characterized in that: In the step (4), the vacuum degassing time is 5 to 30 minutes.

9. The high-performance epoxy resin adhesive based on boron trifluoride monoethylamine according to claim 1, wherein the method of using the adhesive comprises using the adhesive after light or heat curing, wherein the conditions of the light or heat curing comprise: The light wavelength is 315-400nm, the irradiation time is 1-2min; the temperature is 80-120℃, and the time is 2-6h.

Citation Information

Patent Citations

  • Dual-curing adhesive composition and application thereof and method for bonding substrates

    CN103087640A

  • Epoxy adhesive composition having high tg, high adhesion and aging resistance, and preparation method therefor and use thereof

    WO2023236349A1