Closed-loop recyclable solvent-free bio-based adhesive as well as preparation method and application thereof
Covalently crosslinked solvent-free biobased adhesive is formed through the condensation reaction of lipoic acid and tri(2-aminoethyl)amine, which solves the problem of insufficient binding strength and cohesion of biobased adhesives and achieves high shear Its strength and solvent resistance are realized, and the reusable adhesive and closed-loop recycling are achieved, reducing resource waste and environmental pollution.
Patent Information
- Application Number
- CN202411198796.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-29
AI Technical Summary
The binding strength and cohesion of existing bio-based adhesives are weak, and high crosslinked polymers are difficult to recover, resulting in waste of resources and environmental pollution.
Lipoic acid and tri(2-aminoethyl)amine are used to form a covalent crosslinked reusable solvent-free biobased binder through the condensation reaction between the carboxyl and the amino group, using reversible covalent amide bonds at 100- The closed-loop recyclable adhesive was synthesized at 150°C.
The excellent shear strength and solvent resistance of the adhesive are achieved, the shear strength can reach 16.1MPa, and can be reused and closed-loop chemical recovery, the recovery rate of lipoic acid monomer reaches 86%, and tris(2-aminoethyl )amine monomer recovery rate is 90%.
Smart Images

Figure CN118931474A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of bio-based adhesives, and in particular relates to a closed-loop recyclable solvent-free bio-based adhesive and a preparation method and application thereof. Background Art
[0002] Sustainability is becoming increasingly important in the chemical industry and human society due to factors such as dwindling petroleum resources, environmental issues, and the need for customized long-term solutions. A promising approach is to find alternative, renewable raw materials, reduce waste and emissions, and adopt environmentally friendly manufacturing processes. The field of adhesive materials has shifted from fossil fuel-based to bio-based, extracted from plant oils, proteins, sugars and other renewable resources. In ancient times, early humans used natural substances extracted from plants and animals, such as plant resins, tars, and beeswax, to bond objects together. In modern society, the Industrial Revolution brought major advances in adhesive technology, promoting the development of synthetic adhesives with multifunctionality and high performance, such as epoxies and acrylics. Although modern adhesives are widely used and effective, they also bring environmental impacts and health issues, such as resource depletion, volatile organic compounds (VOCs), toxicity, non-renewable resource dependence, and long-term degradation.
[0003] Bio-based adhesives represent an innovative adhesive technology by combining renewable natural materials with unique properties of molecular interactions. Despite the progress, the bond strength of current bio-based adhesives is still relatively weak compared to traditional synthetic adhesives due to the inherent weakness of non-covalent interactions. Currently, significant research efforts are directed towards improving the bonding properties of adhesives, especially by enhancing their adhesion and cohesive strength. Adhesion refers to the bonding strength of the interface between the adhesive and the adherend, which is usually enhanced by chemically modifying specific functional groups. On the other hand, cohesion refers to the intrinsic mechanical strength of the adhesive itself, which is usually fine-tuned by changing non-covalent interactions, such as hydrogen bonding, metal ligand coordination, and host-guest interactions. Non-covalent interactions tend to lead to soft networks of polymers, so covalent interactions are usually introduced to enhance the network hardness of the polymer. It is well known that the crosslinking density of polymers has a profound impact on the mechanical strength of the material.
[0004] The highly cross-linked network structure gives it excellent mechanical properties and a stable structure. This highly cross-linked network is difficult to dissolve in ordinary solvents, and it is also difficult to melt or break at high temperatures. It is almost impractical to recycle highly cross-linked polymers. Therefore, most highly cross-linked polymer materials are discarded after use, which poses a major problem for the sustainable green economy and the environment. Chemical recycling is a plastic recycling method that uses chemical means to convert waste plastics into useful components for utilization. It is not new in principle. The chemical decomposition and depolymerization of polymer compounds have been studied a long time ago, such as the thermal depolymerization of polymethyl methacrylate (PMMA) and polyoxymethylene (CPOM) and the depolymerization reaction of condensation polymers such as nylon (PA) and polyethylene terephthalate (PET). Some of these plastics have been used in factories as an in-process recycling method using chemical methods. In addition, chemical recycling at room temperature makes it easier to depolymerize plastic waste into soluble oligomers or even monomers to regenerate new polymers. Therefore, closed-loop chemical recycling by converting highly cross-linked polymers into monomer feedstocks under certain environmental conditions has great development potential, which can fully restore or even improve the mechanical properties of the recycled polymers, which will play an important role in the circular polymer economy.
[0005] As a bio-based molecule, lipoic acid (TA) contains dynamic disulfide bonds and self-carboxyl groups, and has inherent bonding ability. Therefore, it has the ability to participate in a variety of non-covalent interactions and dynamic reversibility, which is widely recognized, making it the first choice for bio-based adhesive formulations. Tris (2-aminoethyl) amine (TREN) is composed of a nitrogen atom connecting three amino groups to form a trident structure, which provides a good raw material for constructing a three-dimensional network structure with high cross-linking density. Summary of the invention
[0006] In view of the above problems, the object of the present invention is to provide a closed-loop recyclable solvent-free bio-based adhesive and a preparation method and application thereof.
[0007] The present invention is based on lipoic acid and tris(2-aminoethyl)amine, through the condensation reaction between carboxyl and amino groups, using triamine as a cross-linking agent, to successfully synthesize a covalently cross-linked, reusable, solvent-resistant bio-based adhesive.
[0008] The specific technical solutions are as follows: A method for preparing a closed-loop recyclable solvent-free bio-based adhesive comprises the following steps: mixing lipoic acid and tri(2-aminoethyl)amine, and then stirring at a temperature of 100-150°C for 2 hours, and synthesizing a closed-loop recyclable solvent-free bio-based adhesive by using a reversible covalent amide bond, wherein the molar ratio of tri(2-aminoethyl)amine to lipoic acid is 0.2-1:1.
[0009] Preferably, the molar ratio of tris(2-aminoethyl)amine to lipoic acid is 0.6:1.
[0010] A closed-loop recyclable solvent-free bio-based adhesive prepared by the preparation method.
[0011] A closed-loop recyclable solvent-free bio-based adhesive is applied, which is coated on a substrate to achieve bonding between substrates. The bonded substrates can be placed in PE, MeCN, DCM, THF, EA, an acidic solution of pH=1, an alkaline solution of pH=14, an aqueous solution or seawater, and the lap shear performance still maintains a shear strength greater than 7MPa.
[0012] Furthermore, the bonded substrate is heated at 100° C., the adhesive on the substrate is recovered, DMSO and TEA are added, stirred until they are completely dissolved and a clear solution is formed, and then deionized water is added to precipitate lipoic acid. The turbid liquid is centrifuged and dried to obtain lipoic acid monomer powder and protonated tris(2-aminoethyl)amine.
[0013] The beneficial effects of the present invention are: 1) The adhesive of the present invention has excellent shear strength, and the shear strength of CBA0.6 can reach 16.1 MPa; 2) The adhesive of the present invention has excellent solvent resistance, especially in MeCN with the strongest polarity, CBA0.6 can achieve an ultra-strong shear strength of 14.5 MPa, which undoubtedly shows that CBA0.6 has good resistance to organic solvents, especially high polarity ones; 3) The adhesive of the present invention is reusable and can be chemically recycled in a closed loop. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 is a schematic diagram of the structure of lipoic acid; Figure 2 is a schematic diagram of the structure of tris(2-aminoethyl)amine; Figure 3 Schematic diagram of overlapping of solvent-free bio-based adhesive (CBA); Figure 4 It is the bonding performance of solvent-free bio-based adhesive (CBA); Figure 5 The solvent resistance and reusability of CBA0.6; Figure 6 The hydrogen nuclear magnetic resonance spectra of the recovered monomer and the unreacted monomer. DETAILED DESCRIPTION
[0015] The present invention is further described below in conjunction with the accompanying drawings and embodiments, but the protection scope of the present invention is not limited thereto.
[0016] Characterization methods: Lap shear test: Figure 3 As shown, an appropriate amount of solvent-free bio-based adhesive (CBA) was applied to the substrate with a coverage area of 10 mm × 20 mm. The test samples were prepared by hot pressing and then cooled to room temperature. The bonding performance was evaluated using a universal tensile testing machine. The structure of lipoic acid is shown in Figure 1 As shown, the structure of tris(2-aminoethyl)amine is as follows Figure 2 As shown, the shear bond strength was determined by dividing the maximum force at failure by the overlapping contact area. At least 10 tests were performed for each sample data set, and the results were averaged to ensure accuracy.
[0017] Tensile test: An appropriate amount of bio-based adhesive was placed in a hot pressing mold and hot pressed into a film (10mm*20mm). It was then cooled to room temperature and the tensile properties were evaluated using a universal stretching machine. Each sample data set was tested at least 10 times and the results were averaged to ensure accuracy.
[0018] Solvent resistance test: The substrate samples bonded with solvent-free bio-based adhesive (CBA) were immersed in different solvents at room temperature for 24 hours for solvent resistance test. After being taken out, lap shear test was carried out immediately without any treatment. Each sample data set was tested at least 10 times, and the results were averaged to ensure accuracy.
[0019] Example 1
[0020] A closed-loop recyclable solvent-free bio-based adhesive (CBAx) was prepared, where x represents the molar ratio of TREN to TA.
[0021] TA and TREN (the molar ratios of TREN to TA were 0.2, 0.4, 0.6, 0.8 and 1.0, respectively) were weighed into a reaction bottle, and the mixture was stirred at 150 °C for 2 h to obtain closed-loop recyclable solvent-free bio-based adhesives, which were labeled as CBA0.2, CBA0.4, CBA0.6, CBA0.8 and CBA1.0, respectively. They can be directly used in adhesion experiments without further purification and separation.
[0022] To investigate the effect of TREN content in adhesive on adhesive bonding strength, lap shear tests were conducted on iron plates with different CBAx ratios, e.g. Figure 4As shown in (a) and (b) ((a) represents the relationship between adhesive displacement and lap shear strength, and the result of (b) is obtained from (a)), when the content of TREN increases to 0.6, the shear strength of CBA increases to 16.1 MPa. This increase may be due to the addition of TREN, which increases the degree of cross-linking of the cross-linked network and enhances the cohesion of the adhesive. When the content of TREN continues to increase from 0.6 to 1.0, the shear strength of CBA decreases to 7.8 MPa. This may be due to the fact that the excess amino group completely reacts all the carboxyl groups of lipoic acid, reducing the non-covalent interaction between the adhesive and the substrate, thereby reducing the bonding strength.
[0023] Tensile tests were performed on iron plates with different CBAx ratios, such as Figure 4 As shown in (c) and (d), when the TREN content increases from 0.2 to 1.0, the tensile strength gradually increases, and the Young's modulus also increases from 60MPa to 698MPa, which indicates that with the increase of the cross-linking agent content, the mechanical properties of the material are gradually enhanced. This also confirms the previous speculation that the improvement of CBA bonding performance is due to the increase in the cross-linking agent TREN content, which enhances the strength of the material.
[0024] Example 2
[0025] Being able to work in different environments is a requirement that high-performance adhesives must meet. Most bio-based adhesives and supramolecular adhesives cannot resist water and organic solvent environments very well. Even excessive colloid immersion will cause swelling, thus affecting its bonding performance. CBA0.6 was used to combine iron sheets immersed in different solvents to conduct lap shear tests to evaluate its solvent resistance, such as organic solvent environments and underwater environments (PE, MeCN, DCM, THF, EA, pH=1 acidic solution, pH=14 alkaline solution, aqueous solution or seawater). After immersion in these solvents for 24 hours, the results are as follows Figure 5As shown in (a) and (b) ((a) represents the relationship between adhesive displacement and lap shear strength, and the result of (b) is obtained from (a)), it can be found that with the increase of polarity, the resistance of CBA0.6 gradually increases. For example, it can reach 11.3MPa, 11.7MPa, 11.8MPa, and 11.9MPa in PE, DCM, THF, and EA, respectively. In MeCN with the strongest polarity, CBA0.6 can reach an ultra-strong shear strength of 14.5 MPa, which undoubtedly shows that CBA0.6 has good resistance to organic solvents, especially high polarity. In addition, the strength in acidic solution (PH=1), aqueous solution, artificial seawater, and alkaline solution (PH=14) also reached 13.6MPa, 12.7MPa, 9.6MPa, and 7.4MPa, respectively. Therefore, the results prove that CBA0.6 has excellent solvent resistance performance, which also shows a broad development prospect for the selection of adhesive solvent resistance performance.
[0026] Example 3
[0027] Repeatability experiment After the conventional lap shear test, the used adhesive CBA0.6 was recovered and re-hot pressed to prepare the sample. After standing at room temperature for 10 minutes until the sample was completely cured, the second shear strength of CBA0.6 was recorded by lap shear test. The above bonding test steps were repeated 8 times to obtain 10 repeated test results of CBA0.6. Each sample data set was tested at least 10 times, and the results were averaged to ensure accuracy.
[0028] like Figure 5 As shown in (c) and (d) ((c) represents the relationship between adhesive displacement and lap shear strength, and the result of (d) is obtained from (c)), even after ten repeated tests, the shear strength of CBA0.6 still remained at 12.1MPa, and it was able to retain 75.2% of the original strength, which undoubtedly shows the excellent reusability of CBA0.6.
[0029] Example 4
[0030] Recycling Experiment According to the properties of the monomers used, TA is insoluble in water but soluble in some organic solvents, while TREN is soluble in water and some organic solvents. The different solubilities of TA and TREN provide a good idea for the recycling design of CBA0.6 adhesive: the used CBA0.6 sample is recovered in the reaction bottle, DMSO and a small amount of TFA are added, and stirred until the solution is completely clear. Deionized water is continued to be added to precipitate TA, while the protonated TREN continues to remain in the solution. After centrifugation and drying of the turbid liquid, lipoic acid monomer powder and protonated tris(2-aminoethyl)amine monomer are obtained.
[0031] The purity of the recovered monomers was evaluated using H NMR spectroscopy. Figure 6 It can be seen that the H NMR spectra of the recovered monomers are basically consistent with those of the unreacted monomers. It is worth noting that the recovery rate of lipoic acid monomers reaches 86%, and the recovery rate of tris(2-aminoethyl)amine monomers is 90%.
Claims
1. A method for preparing a closed-loop recyclable solvent-free bio-based adhesive, characterized in that: The method comprises the following steps: mixing lipoic acid and tri(2-aminoethyl)amine, and then stirring at a temperature of 100-150°C for 2 hours, and synthesizing a closed-loop recyclable solvent-free bio-based adhesive by using a reversible covalent amide bond, wherein the molar ratio of tri(2-aminoethyl)amine to lipoic acid is 0.2-1:
1.
2. The method for preparing a closed-loop recyclable solvent-free bio-based adhesive according to claim 1, characterized in that: The molar ratio of tris(2-aminoethyl)amine to lipoic acid is 0.6:
1.
3. A closed-loop, recyclable, solvent-free bio-based adhesive prepared by the preparation method according to claim 1 or 2.
4. A use of the closed-loop recyclable solvent-free bio-based adhesive as claimed in claim 3, characterized in that: It is coated on the substrate to achieve bonding between the substrates. The bonded substrates can be placed in PE, MeCN, DCM, THF, EA, pH=1 acidic solution, pH=14 alkaline solution, aqueous solution or seawater, and the lap shear performance still maintains a shear strength greater than 7MPa.
5. The use of a closed-loop recyclable solvent-free bio-based adhesive as claimed in claim 4, characterized in that: The bonded substrate is heated at 100° C., the adhesive on the substrate is recovered, DMSO and TEA are added, stirred until they are completely dissolved and a clear solution is formed, and then deionized water is added to precipitate lipoic acid. The turbid liquid is centrifuged and dried to obtain lipoic acid monomer powder and protonated tris(2-aminoethyl)amine.
Citation Information
Patent Citations
Preparation method and application of silicone rubber film with underwater self-healing capability and adhesiveness
CN110591051A
Degradable covalent cross-linked polymer as well as preparation process and application thereof
CN112521601A
Self-healing supramolecular elastomer based on lipoic acid as well as preparation method and application of self-healing supramolecular elastomer
CN116444807A
High-elasticity degradable elastomer material and preparation method thereof
CN116874807A
Preparation method of thioctic acid-based adhesive with high substrate adhesion
CN118291084A