Organosilicone gel composition as well as preparation method and application thereof
The synthesis of methyl vinyl MQ silicone resin by catalyzing solid acid, the Q unit structure and inorganic components of silicone gel are increased, and nitrogen and phosphorus elements are avoided. Combined with epoxy silane tackifiers, the silicone gel is solved at high temperatures The problems of yellowing and oil dissipation have achieved high temperature durability and oil dissipation resistance, and are suitable for potting of IGBT modules.
Patent Information
- Application Number
- CN202411193350.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-28
AI Technical Summary
Existing silicone gels are prone to yellowing and oil dissipation in high temperature environments, and nitrogen and phosphorus-containing compounds cause poisoning of platinum catalysts, affecting their curing and transparency, making it difficult to meet the packaging needs of high-temperature electronic components.
Using methyl vinyl MQ silicone resin as raw material, catalyzed by solid acid, increases the structure ratio of the Q unit of the organic silicone gel and the proportion of inorganic components, avoids N and P elements, and adds epoxy silanes as tackifiers to improve Yellowing resistance and oil dissipation resistance.
It realizes the durability and oil removal resistance of silicone gel under high temperature conditions of 200-230℃, reduces yellowing and improves adhesion, and is suitable for potting of high-temperature IGBT modules.
Smart Images

Figure BDA0005015683710000011 
Figure BDA0005015683710000021 
Figure BDA0005015683710000022
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of organosilicon materials, and in particular to an organosilicon gel composition and a preparation method and application thereof. Background Art
[0002] Insulated gate bipolar transistor (IGBT) is a power semiconductor device composed of bipolar junction transistor (BJT) and insulated gate field effect transistor (MOS). It has significant performance advantages of low driving power and low saturation voltage drop. It plays two major functions of power switch and power conversion in electronic components and is widely used in new energy vehicles, industrial control, white appliances, new energy power generation, rail transportation and other fields. IGBT module circuits are delicate and easily affected by environmental moisture, dust, salt spray or other pollutants and external force vibration, so it needs to be potted with silicone gel for protection. However, most existing silicone gel products have the defects of easy oil precipitation and severe yellowing at high temperature, and the operating temperature is below 200°C.
[0003] CN 115558297 A discloses a high temperature resistant silicone gel for potting, which can work at 200°C and is suitable for packaging electronic components in high temperature environments. However, compounds containing nitrogen and phosphorus are added to component B of the silicone gel. Such compounds are likely to cause platinum catalyst poisoning, resulting in incomplete curing of the silicone gel. At the same time, nitrogen-containing inhibitors are also likely to cause yellowing of the silicone gel under high temperature conditions, affecting transparency. Summary of the invention
[0004] The present invention aims to solve at least one of the above-mentioned technical problems existing in the prior art. To this end, one of the purposes of the present invention is to provide an organosilicon gel composition; the second purpose of the present invention is to provide a method for preparing the organosilicon gel composition; the third purpose of the present invention is to provide an application of the organosilicon gel composition.
[0005] In order to achieve the above object, the technical solution adopted by the present invention is:
[0006] The first aspect of the present invention provides an organic silicone gel composition, comprising the following components in parts by weight:
[0007] Component A:
[0008]
[0009] Component B:
[0010]
[0011]
[0012] The methyl vinyl MQ silicone resin comprises the following raw materials by weight: 90-150 parts of a capping agent, 300-800 parts of a silicate compound, 200-1000 parts of a small molecule organic silicon compound, 10-30 parts by weight of a solid acid catalyst, and 150-300 parts of a solvent.
[0013] Preferably, the organic silicone gel composition comprises the following components in parts by weight:
[0014] Component A:
[0015]
[0016] Component B:
[0017]
[0018] The methyl vinyl MQ silicone resin comprises the following raw materials by weight: 90-150 parts of a capping agent, 300-800 parts of a silicate compound, 200-1000 parts of a small molecule organic silicon compound, 10-30 parts by weight of a solid acid catalyst, and 150-300 parts of a solvent.
[0019] Preferably, the organic silicone gel composition does not contain compounds containing N and P elements.
[0020] Preferably, the mass ratio of component A to component B is (0.5-1.5):1; further preferably, the mass ratio of component A to component B is (0.8-1.2):1.
[0021] Preferably, the vinyl content of the vinyl silicone oil is 0.1-5 wt %.
[0022] Preferably, the viscosity of the vinyl silicone oil at 23° C. is 100-3000 mPa·s.
[0023] Preferably, the vinyl silicone oil includes at least one of terminal vinyl silicone oil, side vinyl silicone oil, and silicone oil containing vinyl groups in both the terminal group and the side chain.
[0024] Preferably, in the raw materials for preparing the methyl vinyl MQ silicone resin, the solvent includes water and an alcohol solvent.
[0025] Preferably, the mass ratio of water to alcohol solvent is 1:(0.25-1).
[0026] Preferably, the alcohol solvent includes at least one of methanol, ethanol, isopropanol, n-butanol and isobutanol.
[0027] Preferably, the end-capping agent includes at least one of hexamethyldisiloxane and tetramethyldivinyldisiloxane; further preferably, the end-capping agent is a compound of hexamethyldisiloxane and tetramethyldivinyldisiloxane, and the mass ratio of hexamethyldisiloxane to tetramethyldivinyldisiloxane is 1:(0.1-10).
[0028] Preferably, the silicate compound includes at least one of methyl orthosilicate, ethyl orthosilicate, propyl orthosilicate, butyl orthosilicate and polyethyl orthosilicate.
[0029] Preferably, the small molecule organic silicon compound includes at least one of dimethylsiloxane mixed ring body, tetramethylcyclotetrasiloxane, vinyl ring body, and linear body silicone oil.
[0030] Preferably, the solid acid catalyst comprises a macroporous strong acid ion exchange resin.
[0031] Preferably, the methyl vinyl MQ silicone resin is prepared by a method comprising the following steps:
[0032] A1, mixing the end-capping agent and the solvent, adding a solid acid catalyst, and heating for reaction;
[0033] A2, adding silicate compound dropwise and heating for reaction;
[0034] A3, adding a small molecule organic silicon compound, collecting the hydrolysis product, heating up for polymerization reaction, removing impurities, and obtaining the methyl vinyl MQ silicone resin.
[0035] Preferably, in step A1, the temperature of the heating reaction is 80-120°C.
[0036] Preferably, in step A1, the heating reaction time is 30-40 minutes.
[0037] Preferably, in step A2, the temperature of the heating reaction is 80-100°C.
[0038] Preferably, in step A2, the heating reaction time is 5-10 hours.
[0039] Preferably, in the step A2, after the heating reaction is completed, the step further includes cooling to room temperature.
[0040] Preferably, in the step A3, after adding the small molecule organosilicon compound, the steps of standing for stratification, removing the acid water layer, and filtering out the solid acid catalyst are also included.
[0041] Preferably, in the step A3, the temperature of the temperature-raising polymerization reaction is 120-160°C.
[0042] Preferably, in step A3, the time of the temperature-raising polymerization reaction is 3-6 hours.
[0043] Preferably, in step A3, the pressure range of the impurity removal is -0.1 to -0.085 MPa.
[0044] Preferably, the impurities removed include water and small molecule organosilicon compounds.
[0045] Preferably, the cross-linking agent comprises hydrogen-containing silicone oil; the hydrogen content of the hydrogen-containing silicone oil is 0.05-0.5 wt %; and the viscosity of the hydrogen-containing silicone oil at 23° C. is 10-100 mPa·s.
[0046] Preferably, the adhesion promoter includes at least one of γ-(2,3-epoxypropyloxy)propyltrimethoxysilane, γ-(2,3-epoxypropyloxy)propyltriethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane and 2-(3,4-epoxycyclohexyl)ethyltriethoxysilane.
[0047] Preferably, the catalyst comprises a platinum catalyst; the concentration of the catalyst is 3000-5000 ppm.
[0048] Preferably, the inhibitor comprises at least one of tetramethyldivinyldisiloxane, tetramethyltetravinylcyclotetrasiloxane, and acetylene cyclohexanol.
[0049] The second aspect of the present invention provides a method for preparing the organic silicone gel composition according to the first aspect of the present invention, comprising the following steps:
[0050] S1, mixing vinyl silicone oil, methyl vinyl MQ silicone resin, a crosslinking agent and a tackifier to obtain component A;
[0051] S2. Mix vinyl silicone oil, methyl vinyl MQ silicone resin, a catalyst and an inhibitor to obtain component B.
[0052] Preferably, in step S1, stirring is performed; the stirring is firstly performed at a rate of 30-40 r / min for 50-70 min, and then stirred under vacuum conditions for 20-40 min.
[0053] Preferably, in step S2, stirring is performed; the stirring is firstly performed at a rate of 30-40 r / min for 50-70 min, and then stirred under vacuum conditions for 20-40 min.
[0054] The third aspect of the present invention provides use of the organic silicone gel composition described in the first aspect of the present invention in IGBT module potting.
[0055] Compared with the prior art, the present invention has the following beneficial effects:
[0056] 1) The organic silicone gel composition provided by the present invention has excellent yellowing resistance and oil precipitation resistance, good high temperature resistance, and can work for a long time under high temperature conditions of 200-230°C; the components do not contain compounds containing N and P elements, which can reduce the yellowing of the organic silicone gel; the raw material methyl vinyl MQ silicone resin is synthesized using solid acid, which can increase the proportion of Q unit structure of the organic silicone gel, improve the three-dimensional network structure, and also increase the proportion of inorganic components, which is beneficial to improving the yellowing resistance and oil precipitation resistance of the organic silicone gel composition;
[0057] 2) The preparation method of the organic silicone gel composition provided by the present invention is simple and suitable for industrial use. By adding epoxy silane as a tackifier, the adhesion of the organic silicone gel to the substrate can be improved;
[0058] 3) The organic silicone gel composition provided by the present invention can be well applied to IGBT module potting under high temperature conditions. BRIEF DESCRIPTION OF THE DRAWINGS
[0059] Figure 1 The color change diagram of the silicone gel composition in Examples 1-5 and Comparative Example 1 after aging at 230° C. for 1000 hours;
[0060] Figure 2 This is a diagram showing the oil separation of the silicone gel composition in Examples 1-5 and Comparative Example 1 after being baked at 125° C. for 500 hours;
[0061] Figure 3 1 is a thermogravimetric analysis diagram of the silicone gel composition in Example 1 and Comparative Example 1. DETAILED DESCRIPTION
[0062] The present invention is further described in detail below by specific examples. Unless otherwise specified, the raw materials, reagents or devices used in the examples and comparative examples can be obtained from conventional commercial sources or can be obtained by prior art methods. Unless otherwise specified, the experiments or test methods are conventional methods in the art.
[0063] 1. The methyl vinyl MQ silicone resin used in the following examples is prepared by the following steps:
[0064] 1) 120 parts by mass of a mixture of hexamethyldisiloxane and tetramethyldivinyldisiloxane (mass ratio 1:1), 150 parts by mass of deionized water, and 75 parts by mass of methanol were added to a reactor, and then 20 parts by mass of a macroporous strong acid ion exchange resin was added, and the mixture was stirred at 100° C. for 35 minutes;
[0065] 2) slowly dropwise adding 550 parts by weight of methyl orthosilicate, stirring and reacting at 90° C. for 7.5 hours, and cooling the product to room temperature;
[0066] 3) Add 600 parts by weight of dimethylsiloxane mixed ring body, let stand to separate layers after mixing, remove the acid water layer, filter out the macroporous strong acid ion exchange resin to obtain a hydrolyzate, heat to 140° C. and perform polymerization reaction for 4.5 hours, remove water and small molecular weight organic silicon compounds under negative pressure of -0.1 to -0.085 MPa to obtain methyl vinyl MQ silicone resin.
[0067] 2. "Parts" in the following examples refer to "parts by mass" unless otherwise specified.
[0068] Example 1
[0069] This embodiment provides a silicone gel composition, the components of which are shown in Table 1:
[0070] Table 1 Components and contents of the silicone gel composition of Example 1
[0071]
[0072] The preparation steps are as follows:
[0073] S1. Vinyl silicone oil, methyl vinyl MQ silicone resin, hydrogen-containing silicone oil and 2-(3,4-epoxycyclohexyl)ethyltriethoxysilane were placed in a stirring kettle, stirred for 60 min at a stirring rate of 35 r / min, and then vacuum-stirred for 30 min to obtain component A;
[0074] S2. Vinyl silicone oil, methyl vinyl MQ silicone resin, platinum catalyst and tetramethyldivinyldisiloxane were put into a stirring kettle, stirred for 60 minutes at a stirring rate of 35 r / min, and then vacuum-stirred for 30 minutes to obtain component B.
[0075] Example 2
[0076] This embodiment provides a silicone gel composition, the components of which are shown in Table 2:
[0077] Table 2 Components and contents of the silicone gel composition of Example 2
[0078]
[0079] The preparation steps are as follows:
[0080] S1. Vinyl silicone oil, methyl vinyl MQ silicone resin, hydrogen-containing silicone oil and γ-(2,3-epoxypropoxy)propyltriethoxysilane were placed in a stirring kettle, stirred for 60 min at a stirring rate of 35 r / min, and then vacuum-stirred for 30 min to obtain component A;
[0081] S2. Vinyl silicone oil, methyl vinyl MQ silicone resin, platinum catalyst and tetramethyltetravinylcyclotetrasiloxane were put into a stirring kettle, stirred for 60 minutes at a stirring rate of 35 r / min, and then vacuum-stirred for 30 minutes to obtain component B.
[0082] Example 3
[0083] This embodiment provides a silicone gel composition, the components of which are shown in Table 3:
[0084] Table 3 Components and contents of the silicone gel composition of Example 3
[0085]
[0086] The preparation steps are as follows:
[0087] S1. Vinyl silicone oil, methyl vinyl MQ silicone resin, hydrogen-containing silicone oil and 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane were placed in a stirring kettle, stirred for 60 min at a stirring rate of 35 r / min, and then vacuum-stirred for 30 min to obtain component A;
[0088] S2. Vinyl silicone oil, methyl vinyl MQ silicone resin, platinum catalyst and acetylene cyclohexanol were put into a stirring kettle, stirred for 60 minutes at a stirring rate of 35 r / min, and then vacuum-stirred for 30 minutes to obtain component B.
[0089] Example 4
[0090] This embodiment provides a silicone gel composition, the components of which are shown in Table 4:
[0091] Table 4 Components and contents of the silicone gel composition of Example 4
[0092]
[0093] The preparation steps are as follows:
[0094] S1. Vinyl silicone oil, methyl vinyl MQ silicone resin, hydrogen-containing silicone oil and 2-(3,4-epoxycyclohexyl)ethyltriethoxysilane were placed in a stirring kettle, stirred for 60 min at a stirring rate of 35 r / min, and then vacuum-stirred for 30 min to obtain component A;
[0095] S2. Vinyl silicone oil, methyl vinyl MQ silicone resin, platinum catalyst and tetramethyldivinyldisiloxane were put into a stirring kettle, stirred for 60 minutes at a stirring rate of 35 r / min, and then vacuum-stirred for 30 minutes to obtain component B.
[0096] Example 5
[0097] This embodiment provides a silicone gel composition, the components of which are shown in Table 5:
[0098] Table 5 Components and contents of the silicone gel composition of Example 5
[0099]
[0100]
[0101] The preparation steps are as follows:
[0102] S1. Vinyl silicone oil, methyl vinyl MQ silicone resin, hydrogen-containing silicone oil and γ-(2,3-epoxypropoxy)propyltrimethoxysilane are placed in a stirring kettle, stirred for 60 minutes at a stirring rate of 35 r / min, and then vacuum-stirred for 30 minutes to obtain component A;
[0103] S2. Vinyl silicone oil, methyl vinyl MQ silicone resin, platinum catalyst and tetramethyltetravinylcyclotetrasiloxane were put into a stirring kettle, stirred for 60 minutes at a stirring rate of 35 r / min, and then vacuum-stirred for 30 minutes to obtain component B.
[0104] Comparative Example 1
[0105] The only difference from Example 1 is that commercially available methyl vinyl MQ silicone resin is used to synthesize the silicone gel composition.
[0106] Performance Testing
[0107] Component A and component B in Examples 1-5 and Comparative Example 1 were mixed at a mass ratio of 1:1 to obtain an organosilicon gel composition, and the organosilicon gel composition in Examples 1-5 and Comparative Example 1 was subjected to the following performance tests.
[0108] 1. Viscosity: Refer to standard GB / T 2794-2013 and test with a rotational viscometer.
[0109] 2. Cone penetration: refer to standard GB / T 269-1991. After keeping constant temperature at 80℃ for 30min, place the sample on the center of the test bench of the cone penetration meter, align the cone tip with the center of the sample, set the cone penetration time to 5 seconds, turn on the test button, and read the instrument value multiplied by 10 to get the cone penetration value.
[0110] 3. Operation time: Refer to standard GB / T 2794-2013. Mix components A and B evenly and pour them into the test container. Control the sample temperature to 23±2℃, start the test timing, record the mixed viscosity at the beginning, and stop timing when the mixed viscosity doubles. The time difference is the operable time.
[0111] 4. Insulation resistance: Refer to the standard IPC-TM-650. After mixing components A and B evenly, apply them on the comb-shaped circuit board with a thickness of about 100μm, keep the temperature at 80℃ for 30min, take it out and cool it to room temperature, and then test it with a high resistance meter Agilent 4339B.
[0112] 5. Oil separation: Place the solidified gel block on oil-absorbing paper and bake at 125℃ for 500h. Take out the gel block and observe the oil separation on the paper.
[0113] The performance test results are shown in Table 6 below:
[0114] Table 6 Performance test results of the silicone gel composition in Examples 1-5 and Comparative Example 1
[0115]
[0116] Table 6 shows the performance test results of the silicone gel compositions in Examples 1-5 and Comparative Example 1. It can be seen from Table 6 that after the silicone gel compositions in Examples 1-5 are aged at 200°C for 1000h, the change in cone penetration of the colloid is small and the good softness is still maintained; the insulation resistance of the silicone gel composition is higher than that of the silicone gel in the prior art, and the colloid has good insulation properties, which can meet the use requirements of high-power, high-heat-generating IGBT modules.
[0117] Figure 1 The color change diagram of the silicone gel composition in Examples 1-5 and Comparative Example 1 after aging at 230° C. for 1000 h, wherein: Figure 1 (a)- Figure 1 (e) respectively correspond to Examples 1-5, Figure 1 (f) represents Comparative Example 1. Figure 1 It can be seen that the silicone gel compositions in Examples 1-5 only slightly yellowed after aging at 230°C for 1000 hours and remained transparent, while the colloid in Comparative Example 1 severely yellowed after aging at 230°C for 1000 hours, indicating that the silicone gel composition provided by the present invention has excellent yellowing resistance and can adapt to operating temperatures above 200°C. The commercially available methyl vinyl MQ silicone resin used in Comparative Example 1 is synthesized by acid catalysis and alkali neutralization in a traditional process, and the residual acid and alkali will affect the heat resistance of the silicone gel.
[0118] Figure 2 The diagram is a diagram of oil separation of the silicone gel composition in Examples 1-5 and Comparative Example 1 after being baked at 125° C. for 500 hours, wherein: Figure 1 (a)- Figure 1 (e) respectively correspond to Examples 1-5, Figure 1 (f) represents Comparative Example 1. Figure 2It can be seen that the silicone gel compositions in Examples 1-5 only slightly precipitate oil after being baked at 125°C for 500 hours, while the colloid in Comparative Example 1 precipitates oil severely after being baked at 125°C for 500 hours, indicating that the silicone gel composition provided by the present invention has excellent anti-oiling property.
[0119] Figure 3 is the thermogravimetric analysis diagram of the silicone gel composition in Example 1 and Comparative Example 1, Figure 3 It can be seen that when the temperature is lower than 450°C, the thermal stabilities of the silicone gel compositions in Example 1 and Comparative Example 1 are basically the same. When the temperature is higher than 450°C, the weight loss of the silicone gel composition in Comparative Example 1 increases and the thermal stability decreases. Compared with Comparative Example 1, the silicone gel composition in Example 1 loses less weight and has relatively better thermal stability under high temperature conditions.
[0120] The organic silicon gel composition provided by the present invention uses homemade methyl vinyl MQ silicone resin as a raw material, and adopts solid acid to synthesize the reinforcing agent methyl vinyl MQ silicone resin, thereby eliminating the steps of alkali neutralization and multiple water washing required when using liquid acid, effectively avoiding the residual acid and alkali from damaging the chemical bonds of the organic silicon gel under high temperature conditions, and also simplifies the synthesis process, which is energy-saving and environmentally friendly. The organic silicon gel composition has excellent yellowing resistance and oil separation resistance, high temperature aging resistance, can adapt to working temperatures above 200°C, and can be well applied to IGBT potting under high temperature conditions.
Claims
1. A silicone gel composition, characterized in that: The composition comprises the following components in parts by weight: Component A: Vinyl silicone oil 70-120 parts; 10-55 parts of methyl vinyl MQ silicone resin; 5-20 parts of cross-linking agent; 1-7 parts of tackifier; Component B: 60-110 parts of vinyl silicone oil; 5-60 parts of methyl vinyl MQ silicone resin; Catalyst 0.5-2 parts; Inhibitor 0.5-2 parts; The methyl vinyl MQ silicone resin comprises the following raw materials by weight: 90-150 parts of a capping agent, 300-800 parts of a silicate compound, 200-1000 parts of a small molecule organic silicon compound, 10-30 parts by weight of a solid acid catalyst, and 150-300 parts of a solvent.
2. The organic silicone gel composition according to claim 1, characterized in that: The organic silicon gel composition does not contain compounds containing N and P elements.
3. The organic silicone gel composition according to claim 1, characterized in that: The mass ratio of component A to component B is (0.5-1.5):
1.
4. The organic silicone gel composition according to claim 1, characterized in that: The vinyl content of the vinyl silicone oil is 0.1-5wt%; And / or, the viscosity of the vinyl silicone oil at 23° C. is 100-3000 mPa·s.
5. The organic silicone gel composition according to claim 1, characterized in that: In the raw materials for preparing the methyl vinyl MQ silicone resin, the end-capping agent includes at least one of hexamethyldisiloxane and tetramethyldivinyldisiloxane; and / or the silicate compound includes at least one of methyl orthosilicate, ethyl orthosilicate, propyl orthosilicate, butyl orthosilicate, and polyethyl silicate; And / or, the small molecule organosilicon compound includes at least one of dimethylsiloxane mixed ring body, tetramethylcyclotetrasiloxane, vinyl ring body, and linear body silicone oil; And / or, the solid acid catalyst comprises a macroporous strong acid ion exchange resin.
6. The organic silicone gel composition according to claim 1, characterized in that: The methyl vinyl MQ silicone resin is prepared by a method comprising the following steps; A1, mixing the end-capping agent and the solvent, adding a solid acid catalyst, and heating for reaction; A2, adding silicate compound dropwise and heating for reaction; A3, adding a small molecule organic silicon compound, collecting the hydrolysis product, heating up for polymerization reaction, removing impurities, and obtaining the methyl vinyl MQ silicone resin.
7. The organic silicone gel composition according to claim 6, characterized in that: In the preparation of the methyl vinyl MQ silicone resin, in the step A1, the heating reaction temperature is 80-120° C. and the time is 30-40 min; And / or, in step A2, the heating reaction temperature is 80-100° C. and the time is 5-10 h; And / or, in the step A3, the temperature of the temperature-raising polymerization reaction is 120-160° C., and the time is 3-6 hours; And / or, in step A3, the pressure range of the impurity removal is -0.1 to -0.085 MPa.
8. The organic silicone gel composition according to claim 1, characterized in that: The crosslinking agent includes hydrogen-containing silicone oil; the hydrogen content of the hydrogen-containing silicone oil is 0.05-0.5wt%; the viscosity of the hydrogen-containing silicone oil at 23° C. is 10-100 mPa·s; And / or, the adhesion promoter includes at least one of γ-(2,3-epoxypropyloxy)propyltrimethoxysilane, γ-(2,3-epoxypropyloxy)propyltriethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, and 2-(3,4-epoxycyclohexyl)ethyltriethoxysilane.
9. The method for preparing the silicone gel composition according to any one of claims 1 to 8, characterized in that: The following steps are involved: S1, mixing vinyl silicone oil, methyl vinyl MQ silicone resin, a crosslinking agent and a tackifier to obtain component A; S2. Mix vinyl silicone oil, methyl vinyl MQ silicone resin, a catalyst and an inhibitor to obtain component B.
10. Use of the organic silicone gel composition according to any one of claims 1 to 8 in IGBT module potting.
Citation Information
Patent Citations
Method for preparing MQ silicone resins
CN101899157A
Preparation method of novel MQ silicone resin
CN106084227A
Organic silicon pouring sealant and preparation method thereof
CN112778968A
High-temperature-resistant organic silica gel and preparation method thereof
CN115558297A