High-temperature-resistant phase change microspheres as well as preparation method and application thereof
High-temperature-resistant phase change microspheres are prepared by modifying composite phase change materials. Using their characteristics of heat absorption and heat exothermic at high temperatures, the high-temperature performance problems of drilling fluid in deep and ultra-deep wells are solved, and the stable temperature reduction of drilling fluid is achieved and cost reduction.
Patent Information
- Application Number
- CN202310531690.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-11
- Publication Date
- 2024-11-12
AI Technical Summary
The performance of existing drilling fluids deteriorates in high temperature environments, making it difficult to meet the needs of deep and ultra-deep wells, and the existing cooling technology has problems such as high energy consumption, high cost, and damage to equipment.
High-temperature-resistant phase change microspheres are prepared using modified composite phase change materials. The high-temperature phase change core material absorbs heat and maintains constant temperature, reduces the temperature of the drilling fluid, and forms a dense shell through nano-silicon dioxide coating to achieve continuous circulation of the drilling fluid. use.
Effectively reduce the circulation temperature of the drilling fluid, improve the stability and high-temperature resistance of the drilling fluid, significantly reduce drilling costs, and meet the high-temperature environment needs of deep wells and ultra-deep wells.
Smart Images

Figure CN118931497A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of drilling fluid, and in particular relates to a high temperature resistant phase change microsphere and a preparation method and application thereof. Background Art
[0002] With the increase of world energy demand and the development of drilling technology, the oil and gas buried in shallow strata can no longer meet the demand, and it has become inevitable to find oil and gas in deep strata. Most of the oil resources in the Tarim, Junggar, Sichuan Basin and other oil fields are buried in deep strata. Under such circumstances, the drilling of deep wells and ultra-deep wells will inevitably become an important development direction of the oil industry in China and even the world.
[0003] In deep and ultra-deep wells, the quality of drilling fluid is the key to the success of the project, the speed of drilling and the cost. Compared with conventional wells, deep wells have higher requirements for the drilling fluid used, especially the high temperature resistance of the drilling fluid, which is the most basic and important property of deep well drilling fluid. The main slurry material for water-based drilling fluid is bentonite. For example, sodium bentonite is used to increase viscosity, reduce filtration loss and improve lubrication performance. High temperature environment will cause the clay in the drilling fluid to disperse and passivate, and the drilling fluid treatment agent to fail, causing the performance of the drilling fluid to deteriorate; and high temperature environment also has a serious negative impact on drilling tools and logging equipment. High temperature will reduce the sealing of downhole tools and seriously shorten the service life of drilling tools. High temperature will also reduce the life of equipment while drilling, thereby increasing production costs.
[0004] In order to solve the problem of high-temperature drilling, high-temperature drilling fluid is required to have the following characteristics: (1) good high-temperature stability, requiring the use of high-quality bentonite or other high-quality soil, the main chain of the treating agent molecule is not easy to degrade at high temperature, the functional group has strong hydrophilicity, and it is not easy to undergo high-temperature dehydration; (2) low solid phase, especially low bentonite content; (3) good lubricity. Due to the large pressure difference at the bottom of deep wells, thick mud cakes are easily formed, which increases the probability of pressure difference sticking. Therefore, good lubricity plays an important role in reducing downhole complexity; (4) appropriate viscosity and cutting force, with good cuttings carrying capacity, thereby ensuring the cleanliness of the bottom of the well; (5) a large density adjustment range, thereby meeting the density requirements of different well sections.
[0005] The development of passive high-temperature resistant drilling fluids is mainly carried out through the following measures: (1) Using oil-based drilling fluids. Compared with water-based drilling fluids, oil-based drilling fluids have the advantages of high-temperature resistance, salt and calcium resistance, good lubricity and less damage to oil and gas layers. However, oil-based drilling fluids are more polluting to the environment and are not suitable for deep water and other environmentally sensitive areas; (2) Adding high-temperature resistant admixtures to the drilling fluid. This method requires the use of a large amount of high-temperature resistant additives and is relatively costly.
[0006] Active drilling fluid cooling technology generally adopts the following measures. (1) Natural cooling: By extending the circulation route of the drilling fluid tank, the purpose of cooling the drilling fluid can be achieved to a certain extent. This method is generally used when the drilling fluid displacement is not large and the temperature of the returned drilling fluid is not too high. This cooling method is completely affected by climatic conditions. It is not effective for deep wells, ultra-deep wells, and high-temperature and high-pressure wells. For natural gas hydrate wells, it cannot meet the requirements of circulating drilling fluid temperature for safe drilling. (2) Low-temperature medium mixed cooling: Add low-temperature solids (such as ice cubes) or liquids to the drilling fluid pool to cool the drilling fluid through mixed heat conduction. This method is generally used for cooling water-based drilling fluid and is easy to obtain low-temperature water sources. It can only be used as an emergency solution. (3) Cooling device forced cooling: When the temperature of the returned drilling fluid is too high, the drilling fluid cooling system must be used for forced cooling. The working principle of the drilling fluid cooling system is mainly based on three methods: air cooling, spraying, and interactive heat exchange. However, the external cooling device requires energy input, which will result in huge energy loss.
[0007] Chinese patent document CN108251066B discloses a polyacrylonitrile-coated paraffin nano phase-change microcapsule and its preparation method. The microcapsule uses alkane phase-change paraffin as the core material and polyacrylonitrile as the shell layer, and is prepared by a dissolution-emulsification-high-temperature spraying method; the phase-change microcapsule has a small particle size, high latent heat, good thermal stability, and can withstand high-temperature heat setting treatment. The high latent heat can effectively regulate the temperature. The high molecular weight polyacrylonitrile is used as the wall material through the dissolution-spraying technology, and the high-temperature resistant phase-change microcapsule is coated with alkane phase-change paraffin. The whole process does not use acrylonitrile monomer, the process is safe and simple, and there is no monomer pollution. However, the compressive strength of this phase-change microcapsule is low, and it is easy to break under high temperature and high pressure environment.
[0008] Chinese patent document CN104559967A discloses an ultra-dense high-temperature resistant saturated brine drilling fluid system, the mass percentage of each component is: 1.5%-4% sodium bentonite; 8%-14% high-temperature resistant sulfonated fluid loss reducer; 2%-3% emulsified asphalt; 2%-3% lubricant; 0.2%-1.5% pH adjuster; 0.2%-1.0% emulsifier; 20%-30% inorganic salt; 20%-40% weighting agent; the rest is water. The drilling fluid system has a high temperature resistance of 200°C, but the high temperature resistant fluid loss agent, high temperature resistant diluent, high temperature resistant stabilizer and other additives used are expensive, and the problem of high temperature at the bottom of the well is not solved, and high temperature resistance requirements are still put forward for drilling equipment and drilling equipment.
[0009] Chinese patent document CN1657587A discloses a method for preparing microcapsules, which uses paraffin as the phase change core material, polystyrene and polyethylene resins as the basic supporting materials, and mixes and wraps them by heating and melting, and then crushes the prepared paraffin-shaped phase change material after cooling, and then uses melamine-modified urea-formaldehyde resin to encapsulate the paraffin-shaped phase change material in microcapsules by in-situ polymerization. The phase change temperature of this microcapsule is adjustable from 0°C to 70°C, and the maximum phase change enthalpy value is 138kJ / kg. However, the phase change temperature of this microcapsule is too low, and the latent heat of phase change is low, which cannot effectively solve the problem of high temperature at the bottom of the well.
[0010] Chinese patent document CN110126385B discloses a high-temperature, high-enthalpy phase change material multi-wall structure microcapsule and preparation method. The shell structure includes three layers, namely, a volume expansion buffer layer, an anti-corrosion layer and a high-temperature resistant strong layer. The material with a thermal decomposition temperature lower than the core material phase transition temperature is used as the volume expansion buffer layer, which can play a place-taking role in the process of low-temperature coating of the outer shell layer. Through high-temperature thermal decomposition, the vacated volume buffers the volume expansion caused by the core material phase transition. The middle layer is the anti-corrosion layer, which needs to be coated with a layer of dense corrosion-resistant material to prevent the molten phase change material from leaking and damaging the substrate in contact with it. The outermost layer is a high-temperature resistant strong layer, which is required to have a certain density, heat resistance and strength, so that the capsule is protected during the embedding and use of the substrate, and its service life and thermal stability are improved. This three-layer structure of the microcapsule results in low thermal conductivity and slow heat conduction rate, which affects the underground heat exchange rate.
[0011] Chinese patent document CN109652028A discloses a method for controlling the temperature of drilling fluid based on phase change materials, and its technical solution is: including the following steps: (1) phase change materials for drilling fluid are selected: phase change materials with suitable phase change temperatures are selected according to the bottom hole temperature, and the phase change temperature point should be selected at a certain point of the wellbore circulation temperature. The closer the phase change temperature of the phase change material is to the bottom hole temperature, the better the temperature control effect is, and the phase change latent heat should be greater than 160 kJ / kg; (2) the preferred phase change material is used as a drilling fluid treatment agent, and the phase change temperature of the high temperature well is preferably between 70°C and 150°C. The phase change material is a crystalline hydrate, a molten salt, a metal alloy, paraffin, a carboxylic acid, an ester or a polymer alcohol, and a shaped phase change material, a microcapsule phase change material or a composite phase change material can also be used. This invention does not determine the phase change wall material, which may cause the core material to melt and flow out, causing pollution to the drilling fluid and the downhole environment.
[0012] Therefore, it is necessary to develop new drilling fluid cooling technology based on the current high-temperature drilling research and form a new high-temperature drilling technology. In addition to the performance of reducing the drilling fluid temperature, the high-temperature drilling fluid system also needs to consider reuse to reduce drilling costs and ensure that subsequent drilling operations proceed quickly.
[0013] As my country accelerates the exploration and development of deep-sea oil and gas resources, high-temperature drilling will face more severe challenges. Although some relevant research on cooling of drilling fluids has been carried out in China, it still cannot fully meet the requirements of drilling operations in high-temperature environments. Therefore, actively studying new high-temperature drilling fluid cooling technologies is of great significance for the development of my country's deep-sea oil and gas resources. Summary of the invention
[0014] In order to solve the above problems in the prior art, the present invention proposes a high-temperature resistant phase change microsphere and a preparation method and application thereof, utilizing the characteristics of the high-temperature phase change core material that absorbs a large amount of heat and maintains a constant temperature during the phase change process to achieve the effect of actively cooling the high-temperature drilling fluid, thereby achieving the purpose of stabilizing the drilling fluid performance and reducing drilling costs.
[0015] In the first aspect, the present invention proposes a high temperature resistant phase change microsphere, which includes a core material and a wall material coated on the outer surface of the core material, wherein the core material of the high temperature resistant phase change microsphere is a modified composite phase change material, and the wall material of the high temperature resistant phase change microsphere is silica.
[0016] As a specific embodiment of the present invention, the composite phase change material includes erythritol, and the particle size of the composite phase change material is 1 to 10 μm.
[0017] As a specific embodiment of the present invention, the high temperature resistant phase change microspheres have a phase change temperature of 120-140°C, a phase change latent heat of 180-210 J / g, a particle size distribution of 20-28 μm, and a density of 900-1200 kg / m 3 .
[0018] In a second aspect, the present invention provides a method for preparing the high temperature resistant phase change microspheres according to the first aspect, comprising the following steps:
[0019] S1: performing hydrophilic treatment on the composite phase change material to obtain a first product;
[0020] S2: treating the first product obtained in step S1 with a silane coupling agent to improve its surface affinity, thereby obtaining a second product, i.e., a modified composite phase change material;
[0021] S3: emulsifying the second product obtained in step S2 under the action of an emulsifier to obtain a third product;
[0022] S4: mixing the third product obtained in step S3 with tetraethyl orthosilicate under the action of a solvent, washing and drying to obtain the high temperature resistant phase change microspheres.
[0023] As a specific embodiment of the present invention, in the step S1, the hydrophilization treatment includes treatment with an oxidizing acid; the oxidizing acid includes at least one of sulfuric acid, nitric acid, and hydrochloric acid, preferably, the oxidizing acid is a compound of concentrated sulfuric acid and concentrated nitric acid; wherein the concentration of concentrated sulfuric acid is 3 mol / L; the concentration of concentrated nitric acid is 5 mol / L; more preferably, concentrated sulfuric acid and concentrated nitric acid are compounded in a volume ratio of (1-4):1; further preferably, concentrated sulfuric acid and concentrated nitric acid are compounded in a volume ratio of 3:1.
[0024] As a specific embodiment of the present invention, in step S1, the hydrophilization treatment conditions include: temperature of 50-70°C, stirring rate of 100-500 r / min, and stirring time of 0.5-5h.
[0025] As a specific embodiment of the present invention, in step S2, the silane coupling agent includes at least one of KH560, KH570, KH602, KH550, and KH706.
[0026] As a specific embodiment of the present invention, in step S2, the surface affinity treatment conditions include: temperature of 50-70°C, stirring rate of 100-500 r / min, and stirring time of 1-10 h.
[0027] As a specific embodiment of the present invention, in step S3, the emulsifier includes at least one of OP-10, sodium dodecylbenzene sulfonate (hereinafter referred to as SDBS), and carboxymethyl cellulose. Preferably, the emulsifier is OP-10, SDBS, and carboxymethyl cellulose compounded according to (2-4): (4-6): (1-3); the added amount of the emulsifier is 7-13% of the mass of the second product.
[0028] As a specific embodiment of the present invention, in step S3, the emulsification reaction conditions include: temperature of 120-150° C., stirring rate of 500-800 r / min, pressure of 1.5-2 MPa, and emulsification reaction time of 1-2 h.
[0029] As a specific embodiment of the present invention, in step S4, the amount of tetraethyl orthosilicate added is 240-320% of the mass of the third product; the solvent is water or ethanol; preferably, the amount of solvent added is 5-8 times the mass of the third product, and the mass ratio of water to ethanol in the solvent is (3-4): (2-4).
[0030] As a specific embodiment of the present invention, in step S4, the mixing conditions include: temperature of 120-150° C., stirring rate of 500-800 r / min, pH of 3-5, and stirring time of 6-8 h.
[0031] Exemplarily, the method for preparing high temperature resistant phase change microspheres comprises the following steps:
[0032] (1) hydrophilizing the composite phase change material: placing the composite phase change material in an oxidizing acid, raising the temperature to 40-70°C, and uniformly stirring at 100-500 r / min for 0.5-5 h. The hydrophilized phase change material is filtered, washed, and dried to obtain the hydrophilized composite phase change material;
[0033] (2) performing affinity treatment on the surface of the modified composite phase change material: placing the hydrophilized composite phase change material obtained in step (1) in a silane coupling agent solution, raising the temperature to 50-70° C., and stirring uniformly at 100-500 r / min for 1-10 h. The surface-treated phase change material is filtered, washed, and dried to obtain the modified composite phase change material;
[0034] (3) placing the modified composite phase change material powder obtained in step (2) in a high-pressure and high-temperature reactor, adding 300-450% deionized water, 2-4% OP-10, 4-6% SDBS, and 1-3% carboxymethyl cellulose in order, heating to 122° C. to 142° C. at a stirring rate of 500-800 r / min, maintaining the pressure at 1.5-2 MPa, and performing an emulsification reaction for 1-2 hours;
[0035] (4) weighing 300-400% deionized water, 240-320% ethyl orthosilicate, and 240-320% anhydrous ethanol in order, mixing them evenly, and adjusting the pH value to 3-5 to obtain a mixed solution; then slowly injecting the mixed solution into a high-temperature and high-pressure reactor through a high-pressure injection pump to mix with the emulsified modified composite phase change material obtained in step (3), with a dropwise addition speed of 0.2-2 mL / min, a stirring rate of 500-800 r / min, and a stirring time of 6-8 h before naturally cooling;
[0036] (5) The reaction product after cooling in step (4) is washed, filtered and then dried at 80-82° C. to obtain the high temperature resistant phase change microspheres of the present invention.
[0037] In a third aspect, the present invention provides the use of the high temperature resistant phase change microspheres described in the first aspect or the high temperature resistant phase change microspheres prepared by the preparation method described in the second aspect in the field of water-based drilling fluids.
[0038] As a specific implementation of the present invention, the mass fraction ratio of the high temperature resistant phase change microspheres in the water-based drilling fluid is 5%-10%.
[0039] As a specific embodiment of the present invention, the high temperature resistant phase change microspheres are added to the water-based drilling fluid, which can reduce the circulation temperature of the water-based drilling fluid. The reduction value of the circulation temperature of the drilling fluid is 8-12°C.
[0040] As a specific embodiment of the present invention, the high temperature resistant phase change microspheres can be reused, and have significant effects and advantages when used in high temperature and ultra-high temperature environments such as deep wells, ultra-deep wells, geothermal wells, and the reuse rate is ≥90%.
[0041] As a specific embodiment of the present invention, the high temperature resistant phase change microspheres have a breakage rate of less than 5% at 200°C to 220°C and 80 to 120 MPa, and have good stability and high temperature resistance.
[0042] As a specific embodiment of the present invention, the high temperature resistant phase change microspheres have a phase change temperature change value within 2°C after 500 cycles of phase change, and the phase change latent heat loss rate is kept below 10%, and have good thermal stability.
[0043] As a specific embodiment of the present invention, the high temperature resistant phase change microspheres have a small and uniform particle size and a high sphericity. They can smoothly pass through a 100-mesh drilling fluid vibrating screen and re-enter the drilling fluid circulation pool. They can be used continuously and repeatedly without interruption, meeting the requirements for continuous circulation of drilling fluid on site.
[0044] As a specific embodiment of the present invention, the high temperature resistant phase change microspheres have no adverse effect on the filtration loss and rheological properties of the water-based drilling fluid. The high temperature resistant phase change microspheres can be directly added to the water-based drilling fluid system and mixed evenly before use. They can also be directly added to the drilling fluid tank on site and stirred and mixed before use. The use and mixing are relatively simple and convenient, and are convenient for on-site use.
[0045] The above raw materials in the present invention can be prepared in-house or commercially available, and the present invention is not particularly limited thereto.
[0046] Compared with the prior art, the present invention has the following beneficial effects:
[0047] 1. The high temperature resistant phase change microspheres of the present invention are modified by treating the organic polymer phase change material so that it has a higher phase change temperature and latent heat of phase change; the modified composite phase change material is hydrophilicized to make the phase change material more hydrophilic and more conducive to encapsulation. The phase change microspheres are made more resistant to high temperatures by optimizing the dispersant, temperature, and polymerization time in the in-situ polymerization method. The nano-silicon dioxide self-assembly deposition method is adopted to achieve controllable particle size of the phase change microspheres, and the formed shell is denser, meeting the continuous circulation requirements of the drilling fluid. The prepared high temperature resistant phase change microspheres, the phase change core material of the microspheres is the modified composite phase change material, and the wall material of the microspheres is silicon dioxide.
[0048] 2. The high-temperature phase-change isothermal microspheres of the present invention absorb and release heat only within a very small temperature range near their phase-change temperature point, and their phase-change latent heat is relatively large, the phase-change temperature is between 120 and 140°C, and the phase-change latent heat is between 180 and 210 J / g, so they can cool high-temperature drilling fluids with a good cooling effect.
[0049] 3. The high temperature resistant phase change microspheres of the present invention have the characteristics of better sphericity, finer particles and more uniform particle size distribution, and can better meet the requirements of continuous circulation of on-site drilling fluid.
[0050] 4. The high temperature resistant phase change microspheres obtained by microsphere encapsulation and other means in the present invention have a good recovery rate, which can reach 90%.
[0051] 5. The high-temperature drilling fluid based on the high-temperature resistant phase change microspheres of the present invention absorbs heat when the temperature rises to near the melting point, and automatically releases heat after the drilling fluid circulates out of the wellbore, has good reusability and high recovery rate, and can significantly reduce drilling costs. BRIEF DESCRIPTION OF THE DRAWINGS
[0052] Figure 1 This is the cooling curve of the high temperature resistant phase change microspheres obtained in Example 5 of the present invention after being subjected to a cooling and heating cycle. DETAILED DESCRIPTION
[0053] The present invention will be further described below in conjunction with specific embodiments, but they do not constitute any limitation to the present invention.
[0054] The composite phase change material in each embodiment of the present invention is erythritol, which was purchased from Shandong Xingguang Shouchuang Biotechnology Co., Ltd., brand: Shouchuang Biotechnology.
[0055] In each embodiment of the present invention, the formula of the water-based drilling fluid is not specifically specified and can be conventionally selected by those skilled in the art.
[0056] The experimental method used in each embodiment of the present invention is as follows: the reservoir drilling fluid is prepared according to the standard GB / T16783.1-2014 "Drilling fluid field test part 1 water-based drilling fluid", and the performance of the drilling fluid system is tested with reference to the standard GB / T29170-2012 "Petroleum and natural gas industry drilling fluid laboratory test".
[0057] All "parts" described in Examples and Test Examples are "parts by mass".
[0058] The raw materials used in the examples are all conventional commercially available products.
[0059] The concentration of concentrated sulfuric acid used in the examples is 3 mol / L; the concentration of concentrated nitric acid is 5 mol / L.
[0060] Example 1
[0061] This embodiment provides a high temperature resistant phase change microsphere and a preparation method thereof, the specific details are as follows:
[0062] 100 parts of the composite phase change material were weighed and placed in a mixed oxidizing acid, in which the volume ratio of concentrated sulfuric acid to concentrated nitric acid was 3:1. The temperature was raised to 60°C and stirred evenly at 200 r / min for 2 hours. The phase change material after oxidation treatment was filtered, washed and dried to obtain a modified composite phase change material. 100 parts of the modified composite phase change material were placed in a silane coupling agent KH570 solution, the temperature was raised to 60°C and stirred evenly at 200 r / min for 6 hours. The surface-treated composite phase change material was filtered, washed and dried to obtain a hydrophilic modified composite phase change material. 100 parts of the hydrophilic modified composite phase change material powder were placed in a high-pressure and high-temperature reactor, and 3 00 parts of deionized water, 3 parts of OP-10, 5 parts of SDBS, and 2 parts of carboxymethyl cellulose are heated to 122°C at a stirring rate of 500r / min, the pressure is maintained at 1.5MPa, and the dispersion reaction is carried out for 1 hour; 300 parts of deionized water, 300 parts of tetraethyl orthosilicate, and 300 parts of anhydrous ethanol are weighed in a container in sequence, mixed evenly, the pH is adjusted to 4, and then the mixed solution is slowly injected into a high-temperature and high-pressure reactor by a high-pressure injection pump with stirring, the dropwise addition speed is 0.2mL / min, the stirring time is 6h, and it is cooled naturally; the cooled reaction solution is washed, filtered, and then dried at 80°C to prepare high-temperature resistant phase change microspheres, which are recorded as S1.
[0063] Example 2
[0064] This embodiment provides a high temperature resistant phase change microsphere and a preparation method thereof, the specific details are as follows:
[0065] 100 parts of the composite phase change material were weighed and placed in a mixed oxidizing acid, in which the volume ratio of concentrated sulfuric acid to concentrated nitric acid was 3:1. The temperature was raised to 60°C and stirred evenly at 200 r / min for 2 hours. The phase change material after oxidation treatment was filtered, washed and dried to obtain a modified composite phase change material. 100 parts of the modified composite phase change material were placed in a silane coupling agent KH570 solution, the temperature was raised to 60°C and stirred evenly at 200 r / min for 6 hours. The surface-treated composite phase change material was filtered, washed and dried to obtain a hydrophilic modified composite phase change material. 100 parts of the hydrophilic modified composite phase change material powder were placed in a high-pressure and high-temperature reactor, and 3 20 parts of deionized water, 2 parts of OP-10, 5 parts of SDBS, and 2 parts of carboxymethyl cellulose are heated to 122°C at a stirring rate of 500 r / min, the pressure is maintained at 1.5 MPa, and the dispersion reaction is carried out for 1 hour; 320 parts of deionized water, 240 parts of ethyl orthosilicate, and 240 parts of anhydrous ethanol are weighed in a container in turn, mixed evenly, the pH is adjusted to 3, and then the mixed solution is slowly injected into a high-temperature and high-pressure reactor through a high-pressure injection pump and stirred, the dropwise addition speed is 0.4 mL / min, the stirring time is 6 hours, and it is naturally cooled; the cooled reaction solution is washed, filtered, and then dried at 80°C to prepare high-temperature resistant phase change microspheres, which are recorded as S2.
[0066] Example 3
[0067] This embodiment provides a high temperature resistant phase change microsphere and a preparation method thereof, the specific details are as follows:
[0068] 100 parts of the composite phase change material were weighed and placed in a mixed oxidizing acid, in which the volume ratio of concentrated sulfuric acid to concentrated nitric acid was 3:1. The temperature was raised to 60°C and stirred evenly at 200 r / min for 2 hours. The phase change material after oxidation treatment was filtered, washed and dried to obtain a modified composite phase change material. 100 parts of the modified composite phase change material were placed in a silane coupling agent KH560 solution, the temperature was raised to 60°C and stirred evenly at 200 r / min for 6 hours. The surface-treated composite phase change material was filtered, washed and dried to obtain a hydrophilic modified composite phase change material. 100 parts of the hydrophilic modified composite phase change material powder were placed in a high-pressure and high-temperature reactor, and 3 40 parts of deionized water, 5 parts of OP-10, 5 parts of SDBS, and 2 parts of carboxymethyl cellulose are heated to 122°C at a stirring rate of 500 r / min, the pressure is maintained at 1.5 MPa, and the dispersion reaction is carried out for 1 hour; 340 parts of deionized water, 260 parts of ethyl orthosilicate, and 260 parts of anhydrous ethanol are weighed in a container in turn, mixed evenly, the pH is adjusted to 3, and then the mixed solution is slowly injected into a high-temperature and high-pressure reactor by a high-pressure injection pump with stirring, the dropwise addition rate is 0.6 mL / min, the stirring time is 6 hours, and it is naturally cooled; the cooled reaction solution is washed, filtered, and then dried at 80°C to prepare high-temperature resistant phase change microspheres, which are recorded as S3.
[0069] Example 4
[0070] This embodiment provides a high temperature resistant phase change microsphere and a preparation method thereof, the specific details are as follows:
[0071] 100 parts of the composite phase change material were weighed and placed in a mixed oxidizing acid, in which the volume ratio of concentrated sulfuric acid to concentrated nitric acid was 3:1. The temperature was raised to 60°C and stirred evenly at 200 r / min for 2 hours. The phase change material after oxidation treatment was filtered, washed and dried to obtain a modified composite phase change material. 100 parts of the modified composite phase change material were placed in a silane coupling agent KH550 solution, the temperature was raised to 60°C and stirred evenly at 200 r / min for 6 hours. The surface-treated composite phase change material was filtered, washed and dried to obtain a hydrophilic modified composite phase change material. 100 parts of the hydrophilic modified composite phase change material powder were placed in a high-pressure and high-temperature reactor, and 3 00 parts of deionized water, 3 parts of OP-10, 4 parts of SDBS, and 2 parts of carboxymethyl cellulose are heated to 122°C at a stirring rate of 500r / min, the pressure is maintained at 1.5MPa, and the dispersion reaction is carried out for 1 hour; 360 parts of deionized water, 280 parts of ethyl orthosilicate, and 280 parts of anhydrous ethanol are weighed in a container in turn, mixed evenly, the pH is adjusted to 5, and then the mixed solution is slowly injected into a high-temperature and high-pressure reactor by a high-pressure injection pump and stirred, the dropwise addition speed is 0.8mL / min, the stirring time is 6h, and it is cooled naturally; the cooled reaction solution is washed, filtered, and then dried at 80°C to prepare high-temperature resistant phase change microspheres, which are recorded as S4.
[0072] Example 5
[0073] This embodiment provides a high temperature resistant phase change microsphere and a preparation method thereof, the specific details are as follows:
[0074] 100 parts of the composite phase change material were weighed and placed in a mixed oxidizing acid, in which the volume ratio of concentrated sulfuric acid to concentrated nitric acid was 3:1. The temperature was raised to 60°C and stirred evenly at 200 r / min for 2 hours. The phase change material after oxidation treatment was filtered, washed and dried to obtain a modified composite phase change material. 100 parts of the modified composite phase change material were placed in a silane coupling agent KH602 solution, the temperature was raised to 60°C and stirred evenly at 200 r / min for 6 hours. The surface-treated composite phase change material was filtered, washed and dried to obtain a hydrophilic modified composite phase change material. 100 parts of the hydrophilic modified composite phase change material powder were placed in a high-pressure and high-temperature reactor, and 4 00 parts of deionized water, 3 parts of OP-10, 6 parts of SDBS, and 2 parts of carboxymethyl cellulose are heated to 122°C at a stirring rate of 500r / min, the pressure is maintained at 1.5MPa, and the dispersion reaction is carried out for 1 hour; 360 parts of deionized water, 320 parts of ethyl orthosilicate, and 320 parts of anhydrous ethanol are weighed in a container in turn, mixed evenly, the pH is adjusted to 5, and then the mixed solution is slowly injected into a high-temperature and high-pressure reactor by a high-pressure injection pump and stirred, the dropwise addition speed is 1.0mL / min, the stirring time is 6h, and it is naturally cooled; the cooled reaction liquid is washed, filtered, and then dried at 80°C to prepare high-temperature resistant phase change microspheres, which are recorded as S5.
[0075] Example 6
[0076] This embodiment provides a high temperature resistant phase change microsphere and a preparation method thereof, the specific details are as follows:
[0077] 100 parts of the composite phase change material were weighed and placed in a mixed oxidizing acid, in which the volume ratio of concentrated sulfuric acid to concentrated nitric acid was 3:1. The temperature was raised to 60°C and stirred evenly at 200 r / min for 2 hours. The phase change material after oxidation treatment was filtered, washed and dried to obtain a modified composite phase change material. 100 parts of the modified composite phase change material were placed in a silane coupling agent KH550 solution, the temperature was raised to 60°C and stirred evenly at 200 r / min for 6 hours. The surface-treated composite phase change material was filtered, washed and dried to obtain a hydrophilic modified composite phase change material. 100 parts of the hydrophilic modified composite phase change material powder were placed in a high-pressure and high-temperature reactor, and 4 50 parts of deionized water, 3 parts of OP-10, 5 parts of SDBS, and 1 part of carboxymethyl cellulose are heated to 122°C at a stirring rate of 500 r / min, the pressure is maintained at 1.5 MPa, and the dispersion reaction is carried out for 1 hour; 400 parts of deionized water, 320 parts of tetraethyl orthosilicate, and 320 parts of anhydrous ethanol are weighed in a container in turn, mixed evenly, the pH is adjusted to 5, and then the mixed solution is slowly injected into a high-temperature and high-pressure reactor by a high-pressure injection pump with stirring, the dropwise addition rate is 1.2 mL / min, the stirring time is 6 hours, and it is cooled naturally; the cooled reaction solution is washed, filtered, and then dried at 80°C to prepare high-temperature resistant phase change microspheres, which are recorded as S6.
[0078] Example 7
[0079] This embodiment provides a high temperature resistant phase change microsphere and a preparation method thereof, the specific details are as follows:
[0080] 100 parts of the composite phase change material were weighed and placed in a mixed oxidizing acid, in which the volume ratio of concentrated sulfuric acid to concentrated nitric acid was 3:1. The temperature was raised to 60°C and stirred evenly at 200 r / min for 2 hours. The phase change material after oxidation treatment was filtered, washed and dried to obtain a modified composite phase change material. 100 parts of the modified composite phase change material were placed in a silane coupling agent KH792 solution, the temperature was raised to 60°C and stirred evenly at 200 r / min for 6 hours. The surface-treated composite phase change material was filtered, washed and dried to obtain a hydrophilic modified composite phase change material. 100 parts of the hydrophilic modified composite phase change material powder were placed in a high-pressure and high-temperature reactor, and 4 50 parts of deionized water, 3 parts of OP-10, 5 parts of SDBS, and 3 parts of carboxymethyl cellulose are heated to 122°C at a stirring rate of 500 r / min, the pressure is maintained at 1.5 MPa, and the dispersion reaction is carried out for 1 hour; 400 parts of deionized water, 320 parts of ethyl orthosilicate, and 320 parts of anhydrous ethanol are weighed in a container in turn, mixed evenly, the pH is adjusted to 5, and then the mixed solution is slowly injected into a high-temperature and high-pressure reactor by a high-pressure injection pump with stirring, the drop rate is 1.2 mL / min, the stirring time is 6 hours, and it is cooled naturally; the cooled reaction solution is washed, filtered, and then dried at 80°C to prepare high-temperature resistant phase change microspheres, which are recorded as S7.
[0081] Example 8
[0082] This embodiment provides a high temperature resistant phase change microsphere and a preparation method thereof, the specific details are as follows:
[0083] 100 parts of the composite phase change material were weighed and placed in a mixed oxidizing acid, in which the volume ratio of concentrated sulfuric acid to concentrated nitric acid was 3:1. The temperature was raised to 60°C and stirred evenly at 200 r / min for 2 hours. The phase change material after oxidation treatment was filtered, washed and dried to obtain a modified composite phase change material. 100 parts of the modified composite phase change material were placed in a silane coupling agent KH900 solution, the temperature was raised to 60°C and stirred evenly at 200 r / min for 6 hours. The surface-treated composite phase change material was filtered, washed and dried to obtain a hydrophilic modified composite phase change material. 100 parts of the hydrophilic modified composite phase change material powder were placed in a high-pressure and high-temperature reactor, and 4 50 parts of deionized water, 3 parts of OP-10, 5 parts of SDBS, and 2 parts of carboxymethyl cellulose are heated to 122°C at a stirring rate of 500 r / min, the pressure is maintained at 1.5 MPa, and the dispersion reaction is carried out for 1 hour; 380 parts of deionized water, 320 parts of ethyl orthosilicate, and 320 parts of anhydrous ethanol are weighed in a container in turn, mixed evenly, the pH is adjusted to 4, and then the mixed solution is slowly injected into a high-temperature and high-pressure reactor by a high-pressure injection pump and stirred, the dropwise addition speed is 1.2 mL / min, the stirring time is 6 hours, and it is naturally cooled; the cooled reaction solution is washed, filtered, and then dried at 80°C to prepare high-temperature resistant phase change microspheres, which are recorded as S8.
[0084] Comparative Example 1
[0085] The high temperature resistant phase change microspheres were prepared in the same manner as in Example 1.
[0086] The difference is that no affinity treatment is performed during the preparation of the high temperature resistant phase change microsphere core material.
[0087] 100 parts of the composite phase change material were weighed and placed in a mixed oxidizing acid, in which the volume ratio of concentrated sulfuric acid to concentrated nitric acid was 3:1. The temperature was raised to 60°C and stirred evenly at 200 r / min for 2 hours. The phase change material after oxidation treatment was filtered, washed and dried to obtain a modified composite phase change material. 100 parts of the modified composite phase change material powder were placed in a high-pressure and high-temperature reactor, and 300 parts of deionized water, 3 parts of OP-10, 5 parts of SDBS and 2 parts of carboxymethyl cellulose were weighed in turn. The mixture was stirred at a rate of 500 r / min. , heat to 122°C, maintain the pressure at 1.5MPa, and disperse the reaction for 1 hour; weigh 300 parts of deionized water, 300 parts of ethyl orthosilicate, and 300 parts of anhydrous ethanol in a container, mix them evenly, adjust the pH to 4, and then slowly inject the mixed solution into the high-temperature and high-pressure reactor through a high-pressure injection pump with stirring, the dropwise addition rate is 0.2mL / min, the stirring time is 6h, and it is cooled naturally; the cooled reaction solution is washed, filtered, and then dried at 80°C to prepare high-temperature resistant phase change microspheres, which are recorded as DS1.
[0088] Comparative Example 2
[0089] The high temperature resistant phase change microspheres were prepared in the same manner as in Example 1.
[0090] The difference is that no hydrophilic treatment is performed during the preparation of the high temperature resistant phase change microsphere core material.
[0091] 100 parts of the composite phase change material were weighed and placed in a silane coupling agent KH570 solution, the temperature was raised to 60°C, and the mixture was stirred evenly at 200 r / min for 6 hours. The surface-treated composite phase change material was filtered, washed, and dried to obtain a hydrophilic modified composite phase change material. 100 parts of the hydrophilic modified composite phase change material powder were placed in a high-pressure and high-temperature reactor, and 300 parts of deionized water, 3 parts of OP-10, 5 parts of SDBS, and 2 parts of carboxymethyl cellulose were weighed in sequence. The mixture was heated at a stirring rate of 500 r / min. The temperature was raised to 122°C, the pressure was maintained at 1.5 MPa, and the dispersion reaction was carried out for 1 hour; 300 parts of deionized water, 300 parts of ethyl orthosilicate, and 300 parts of anhydrous ethanol were weighed in a container in turn, mixed evenly, the pH was adjusted to 4, and then the mixed solution was slowly injected into the high-temperature and high-pressure reactor by a high-pressure injection pump with stirring, the dropwise addition rate was 0.2 mL / min, the stirring time was 6 hours, and it was cooled naturally; the cooled reaction solution was washed, filtered, and dried at 80°C to prepare high-temperature resistant phase change microspheres, which were recorded as DS1.
[0092] Comparative Example 3
[0093] The high temperature resistant phase change microspheres were prepared in the same manner as in Example 1.
[0094] The difference is that the pH value is controlled to be 9 when tetraethyl orthosilicate is added.
[0095] 100 parts of the composite phase change material were weighed and placed in a mixed oxidizing acid, in which the volume ratio of concentrated sulfuric acid to concentrated nitric acid was 3:1. The temperature was raised to 60°C and stirred evenly at 200 r / min for 2 hours. The phase change material after oxidation treatment was filtered, washed and dried to obtain a modified composite phase change material. 100 parts of the modified composite phase change material were placed in a silane coupling agent KH570 solution, the temperature was raised to 60°C and stirred evenly at 200 r / min for 6 hours. The surface-treated composite phase change material was filtered, washed and dried to obtain a hydrophilic modified composite phase change material. 100 parts of the hydrophilic modified composite phase change material powder were placed in a high-pressure and high-temperature reactor, and 3 00 parts of deionized water, 3 parts of OP-10, 5 parts of SDBS, and 2 parts of carboxymethyl cellulose are heated to 122°C at a stirring rate of 500r / min, the pressure is maintained at 1.5MPa, and the dispersion reaction is carried out for 1 hour; 300 parts of deionized water, 300 parts of tetraethyl orthosilicate, and 300 parts of anhydrous ethanol are weighed in a container in turn, mixed evenly, the pH is adjusted to 9, and then the mixed solution is slowly injected into a high-temperature and high-pressure reactor by a high-pressure injection pump with stirring, the dropwise addition speed is 0.2mL / min, the stirring time is 6h, and it is cooled naturally; the cooled reaction liquid is washed, filtered, and then dried at 80°C to prepare high-temperature resistant phase change microspheres, which are recorded as DS1.
[0096] Test Example 1
[0097] The phase change temperature, phase change latent heat, and particle size of Examples 1-8 and Comparative Examples 1-3 were tested by METTLER differential scanning calorimeter and laser particle size analyzer, respectively. The test results are shown in Table 1.
[0098] Table 1 Performance test of high temperature resistant phase change microspheres
[0099]
[0100]
[0101] The experimental results show that the high temperature resistant phase change microspheres prepared by the present invention have the advantages of better phase change temperature, larger phase change latent heat, more uniform and smaller particle size, and are more suitable for cooling high temperature drilling fluid.
[0102] Test Example 2
[0103] The effects of adding different mass fractions of high temperature resistant phase change microspheres of Example 1 and Comparative Example 3 on the circulation temperature of high temperature water-based drilling fluid were tested by an indoor drilling simulation circulation experimental device.
[0104] The specific method for preparing high-temperature water-based drilling fluid is as follows: put 100 parts of water into a stirring container, add 6 parts of sodium bentonite while stirring, continue stirring for 25 minutes, stop stirring, and seal and cure for more than 24 hours to obtain a prehydrated bentonite slurry; under high-speed stirring at a speed of 10,000 rpm, add 0.3 parts of Na2CO3, 6 parts of lignite resin filtrate reducer, 3.6 parts of sulfonated lignite, and 4 parts of lubricant to the prehydrated bentonite slurry in the above proportions, stir each material for 40 minutes, continue stirring for 75 minutes after all are added, and after high-speed stirring for 35 minutes, a high-temperature water-based drilling fluid is obtained.
[0105] First, the high-temperature water-based drilling fluid is heated and circulated until the circulating temperature of the drilling fluid reaches 160°C and stabilizes. Then, different mass fractions of high-temperature resistant phase change microspheres are added to test the maximum reduction value of the circulating temperature. The test results are shown in Table 2.
[0106] Table 2 Cooling performance test of high temperature resistant phase change microspheres
[0107] High temperature resistant phase change microspheres 5% 6% 7% 8% 9% 10% Maximum cooling value of high temperature resistant phase change microsphere S1 8.3 8.9 9.5 10.1 10.9 11.7 Maximum cooling value of high temperature resistant phase change microspheres DS3 4.1 4.9 5.7 6.8 7.3 8.1
[0108] The experimental results show that the high temperature resistant phase change microspheres prepared by the present invention have the best cooling effect on high temperature water-based drilling fluid, which is significantly better than the comparative example.
[0109] Test Example 3
[0110] The effects of the high temperature resistant phase change microspheres prepared in Examples 1-8 and Comparative Examples 1-3 on the filtration performance of high temperature water-based drilling fluids were tested.
[0111] Evaluation experimental method: 100 parts of water were put into a stirring container, and 6 parts of sodium bentonite were added while stirring. After continuing to stir for 25 minutes, stirring was stopped, and the prehydrated bentonite slurry was obtained by sealed curing for more than 24 hours. Under high-speed stirring at a speed of 10,000 rpm, 0.3 parts of Na2CO3, 6 parts of lignite resin filtrate reducer, 3.6 parts of sulfonated lignite, 4 parts of lubricant, and 10 parts of high-temperature resistant phase change microspheres were added to the prehydrated bentonite slurry in the above proportions. Each material was stirred for 40 minutes. After all the materials were added, stirring was continued for 75 minutes. After high-speed stirring for 35 minutes, the changes in the filtration performance of the drilling fluid were compared by a water loss meter. The experimental results are shown in Table 3.
[0112] Table 3 Test on the influence of high temperature resistant phase change microspheres on drilling fluid loss performance
[0113]
[0114] The experimental results show that the high temperature resistant phase change microspheres prepared by the present invention have no effect on the filtration performance of the high temperature water-based drilling fluid. After being added, the filtration performance of the high temperature water-based drilling fluid is slightly improved, and the filtration loss is slightly reduced. Comparative Example 3 has a large particle size, which has a great impact on the filtration performance of the high temperature water-based drilling fluid, and significantly increases the filtration loss.
[0115] Test Example 4
[0116] The effects of the high temperature resistant phase change microspheres prepared in Examples 1-8 and Comparative Examples 1-3 on the rheological properties of high temperature water-based drilling fluids were tested.
[0117] Evaluation experimental method: 100 parts of water were put into a stirring container, and 6 parts of sodium bentonite were added while stirring. After continuing to stir for 25 minutes, stirring was stopped, and the prehydrated bentonite slurry was obtained by sealed curing for more than 24 hours. Under high-speed stirring at a speed of 10,000 rpm, 0.3 parts of Na2CO3, 6 parts of lignite resin filtrate reducer, 3.6 parts of sulfonated lignite, 4 parts of lubricant, and 10 parts of high-temperature resistant phase change microspheres were added to the prehydrated bentonite slurry in the above proportions. Each material was stirred for 40 minutes. After all the materials were added, stirring was continued for 75 minutes. After high-speed stirring for 35 minutes, the rheological properties of the drilling fluid were tested by a rotational viscometer. The experimental results are shown in Table 4.
[0118] Table 4 Test on the influence of high temperature resistant phase change microspheres on the rheological properties of drilling fluid
[0119]
[0120]
[0121] The experimental results show that the high temperature resistant phase change microspheres prepared by the present invention have a relatively uniform and small particle size and a high particle sphericity, and have little effect on the rheological properties of the high temperature water-based drilling fluid. In the comparative example, the particle size is larger, which has a greater effect on the rheological properties of the drilling fluid, and the apparent viscosity and plastic viscosity of the drilling fluid will increase. In particular, the high temperature resistant phase change microspheres in comparative example 2 have a large and uneven particle size, which has a very large effect on the rheological properties of the high temperature water-based drilling fluid, and the thickening is obvious.
[0122] Test Example 5
[0123] The compressive particle size degradation rate and the breakage rate of the high temperature resistant phase change microspheres prepared in Examples 1-8 and Comparative Examples 1-3 were tested.
[0124] After the high temperature resistant phase change microspheres enter the downhole environment with the drilling fluid, when the external force exceeds the compressive strength of the high temperature resistant phase change microspheres, the high temperature resistant phase change microspheres are squeezed and broken, causing the phase change core material to leak. The compressive strength of the high temperature resistant phase change microspheres is evaluated by taking the compressive particle size degradation rate and the crushing rate of the high temperature resistant phase change microspheres as indicators.
[0125] Evaluation experimental method: A high temperature and high pressure reactor was used to pressurize the high temperature resistant phase change microspheres, and the D90, D50, and D10 particle size degradation rates of the high temperature resistant phase change microspheres were tested after stabilizing at 220°C, 80MPa, 100MPa, and 120MPa for 30 minutes. The residue of the high temperature resistant phase change microspheres after being pressed and passing through a 400-mesh standard sieve was weighed, and the crushing rate was calculated. The experimental results are shown in Tables 5, 6, and 7.
[0126] Table 5 Compressive particle size degradation rate and crushing rate of high temperature resistant phase change microspheres (220℃, 80MPa)
[0127]
[0128]
[0129] Table 6 Compressive particle size degradation rate and crushing rate of high temperature resistant phase change microspheres (220℃, 100MPa)
[0130] Serial number S1 S2 S3 S4 S5 S6 S7 S8 DS1 DS2 DS3 D90 degradation rate / % 1.2 1.6 1.8 1.3 0.6 1.3 1.7 1.9 5.3 5.7 6.2 D50 degradation rate / % 2.5 2.7 2.8 2.1 1.1 2.6 2.8 2.9 7.3 7.1 7.5 D10 degradation rate / % 3.3 3.8 3.1 2.9 1.7 3.4 3.9 3.2 9.2 9.5 9.9 Quality loss rate / % 2.1 2.3 2.2 2.1 0.9 2.2 2.4 2.3 4.5 4.1 4.1 Broken rate / % 2.1 2.3 2.2 2.1 0.9 2.2 2.4 2.3 4.5 4.1 4.1
[0131] Table 7 Compressive particle size degradation rate and crushing rate of high temperature resistant phase change microspheres (220℃, 120MPa)
[0132] Serial number S1 S2 S3 S4 S5 S6 S7 S8 DS1 DS2 DS3 D90 degradation rate / % 2.1 2.7 2.9 2.4 1.3 2.2 2.8 3.0 7.3 7.8 7.3 D50 degradation rate / % 3.9 3.5 3.7 3.2 2.1 4.1 3.6 3.8 9.1 9.8 9.7 D10 degradation rate / % 5.1 4.8 4.5 4.6 3.3 5.2 4.9 4.6 11.2 11.5 10.9 Quality loss rate / % 5.3 4.5 5.1 5.2 2.2 5.4 4.6 5.2 7.6 7.2 7.1 Broken rate / % 5.3 4.5 5.1 5.2 2.2 5.4 4.6 5.2 7.6 7.2 7.1
[0133] Test Example 6
[0134] The compressive particle size degradation rate and the breakage rate of the high temperature resistant phase change microspheres prepared in Examples 1-8 and Comparative Examples 1-3 were tested.
[0135] After the high temperature resistant phase change microspheres enter the downhole environment with the drilling fluid, when the external force exceeds the compressive strength of the high temperature resistant phase change microspheres, the high temperature resistant phase change microspheres are squeezed and broken, causing the phase change core material to leak. The compressive strength of the high temperature resistant phase change microspheres is evaluated by taking the compressive particle size degradation rate and the crushing rate of the high temperature resistant phase change microspheres as indicators.
[0136] Evaluation experimental method: The high temperature and high pressure reactor was used to heat the high temperature resistant phase change microspheres, and the D90, D50 and D10 particle size degradation rates of the high temperature resistant phase change microspheres were tested after stabilizing at 200°C, 210°C and 220°C and 120MPa for 30 minutes. The residue of the high temperature resistant phase change microspheres after being pressed and passing through a 400-mesh standard sieve was weighed, and the crushing rate was calculated. The experimental results are shown in Tables 8, 9 and 10.
[0137] Table 8 Compressive particle size degradation rate and crushing rate of high temperature resistant phase change microspheres (200℃, 120MPa)
[0138] Serial number S1 S2 S3 S4 S5 S6 S7 S8 DS1 DS2 DS3 D90 degradation rate / % 1.8 2.4 2.6 2.1 1.0 1.9 2.5 2.7 7.0 7.5 7.0 D50 degradation rate / % 3.6 3.2 3.4 2.9 1.8 3.7 3.3 3.5 8.7 9.5 9.4 D10 degradation rate / % 4.8 4.5 4.2 4.3 3.0 4.9 4.6 4.3 10.9 11.2 10.6 Quality loss rate / % 5.0 4.2 4.8 4.9 1.8 5.1 4.3 4.9 7.3 6.9 6.8 Broken rate / % 5.0 4.2 4.8 4.9 1.8 5.1 4.3 4.9 7.3 6.9 6.8
[0139] Table 9 Compressive particle size degradation rate and crushing rate of high temperature resistant phase change microspheres (210℃, 120MPa)
[0140] Serial number S1 S2 S3 S4 S5 S6 S7 S8 DS1 DS2 DS3 D90 degradation rate / % 2.0 2.5 2.8 2.2 1.1 2.1 2.6 2.9 7.2 7.7 7.1 D50 degradation rate / % 3.8 3.3 3.6 3.0 2.0 3.9 3.4 3.7 8.9 9.7 9.6 D10 degradation rate / % 4.9 4.7 4.4 4.4 3.2 5.1 4.8 4.5 11.0 11.3 10.8 Quality loss rate / % 5.1 4.3 5.0 5.0 2.1 5.2 4.4 5.1 7.4 7.1 6.9 Broken rate / % 5.1 4.3 5.0 5.0 2.1 5.2 4.4 5.1 7.4 7.1 6.9
[0141] Table 10 Compressive particle size degradation rate and crushing rate of high temperature resistant phase change microspheres (220℃, 120MPa)
[0142] Serial number S1 S2 S3 S4 S5 S6 S7 S8 DS1 DS2 DS3 D90 degradation rate / % 2.1 2.7 2.9 2.4 1.3 2.2 2.8 3.1 7.3 7.8 7.3 D50 degradation rate / % 3.9 3.5 3.7 3.2 2.1 4.1 3.6 3.8 9.1 9.8 9.7 D10 degradation rate / % 5.1 4.8 4.5 4.6 3.3 5.2 4.9 4.6 11.2 11.5 10.9 Quality loss rate / % 5.3 4.5 5.1 5.2 2.2 5.4 4.6 5.2 7.6 7.2 7.1 Broken rate / % 5.3 4.5 5.1 5.2 2.2 5.4 4.6 5.2 7.6 7.2 7.1
[0143] The experimental results show that the high temperature resistant phase change microspheres prepared by the present invention have a small particle size degradation rate and a small breakage rate under high temperature and high pressure, and have a high compressive strength.
[0144] Test Example 7
[0145] The thermal stability of the high temperature resistant phase change microspheres prepared in Examples 1-8 and Comparative Examples 1-3 was tested.
[0146] The phase change microspheres were placed in a high and low temperature alternating box, and the high and low temperature cycle program was set: 1) heating to 170°C and maintaining for 25 min; 2) cooling to 120°C and maintaining for 25 min; 3) heating to 170°C and maintaining for 25 min. After cycling this phase change test 500 times, the phase change temperature and phase change latent heat of the phase change microspheres after the cycle were tested. The experimental results are shown in Table 11.
[0147] Table 11 Changes in phase change temperature and phase change latent heat of phase change microspheres before and after cycling
[0148]
[0149] Among them, after the high temperature resistant phase change microspheres obtained in Example 5 were repeatedly heated and cooled, the phase change temperature curve of the product was as follows: Figure 1 shown.
[0150] The experimental results show that after 500 cycles of phase change, the phase change temperature of the high temperature resistant phase change microspheres prepared by the present invention is within 2°C, the phase change latent heat loss rate is below 10%, and it has good thermal stability and is reusable with a reusability of more than 90%.
[0151] In summary, the high temperature resistant phase change microspheres prepared by the present invention can effectively regulate the temperature of high temperature water-based drilling fluid. After adding the high temperature resistant phase change microspheres to the drilling fluid, the characteristics of absorbing heat and maintaining a relatively stable temperature during the phase change process can be utilized to achieve the purpose of reducing the circulating temperature of the water-based drilling fluid in the wellbore, providing a lower working environment for the drilling fluid and downhole tools, which will be conducive to ensuring the safety of deep and ultra-deep high temperature and ultra-high temperature drilling.
[0152] Any numerical value mentioned in the present invention, if there is only an interval of two units between any minimum value and any maximum value, includes all values from the minimum value to the maximum value each time increasing by one unit. For example, if the amount of a component, or the value of a process variable such as temperature, pressure, time, etc. is declared to be 50-90, in this specification it means that 51-89, 52-88... and 69-71 and 70-71 are specifically listed. For non-integer values, 0.1, 0.01, 0.001 or 0.0001 can be appropriately considered as a unit. These are just some specially specified examples. In this application, in a similar manner, all possible combinations of numerical values between the listed minimum and maximum values are considered to have been disclosed.
[0153] It should be noted that the embodiments described above are only used to explain the present invention and do not constitute any limitation to the present invention. The present invention has been described with reference to typical embodiments, but it should be understood that the words used therein are descriptive and explanatory words, rather than restrictive words. The present invention may be modified as specified within the scope of the claims of the present invention, and the present invention may be revised without departing from the scope and spirit of the present invention. Although the present invention described therein relates to specific methods, materials and embodiments, it does not mean that the present invention is limited to the specific examples disclosed therein, on the contrary, the present invention can be extended to all other methods and applications with the same functions.
Claims
1. A high temperature resistant phase change microsphere, characterized in that: The high temperature resistant phase change microspheres include a core material and a wall material coated on the outer surface of the core material, wherein the core material of the high temperature resistant phase change microspheres is a modified composite phase change material, and the wall material of the high temperature resistant phase change microspheres is silicon dioxide.
2. The high temperature resistant phase transition microstructure according to claim 1, characterized in that: The composite phase change material comprises erythritol, and the particle size of the composite phase change material is 1 to 10 μm.
3. The method according to claim 1 or 2, characterized in that: The phase change temperature of the high temperature resistant phase change microspheres is 120-140°C, the phase change latent heat is 180-210 J / g, the particle size distribution is 20-28 μm, and the density is 900-1200 kg / m 3 .
4. A method for preparing high temperature resistant phase change microspheres according to any one of claims 1 to 3, characterized in that: The following steps are involved: S1: performing hydrophilic treatment on the composite phase change material to obtain a first product; S2: treating the first product obtained in step S1 with a silane coupling agent to improve its surface affinity, thereby obtaining a second product, i.e., a modified composite phase change material; S3: emulsifying the second product obtained in step S2 under the action of an emulsifier to obtain a third product; S4: mixing the third product obtained in step S3 with tetraethyl orthosilicate under the action of a solvent, washing and drying to obtain the high temperature resistant phase change microspheres.
5. The preparation method according to claim 4, characterized in that: In the step S1, the hydrophilization treatment includes treatment with an oxidizing acid; the oxidizing acid includes at least one of sulfuric acid, nitric acid, and hydrochloric acid, and the hydrophilization treatment conditions include: a temperature of 50-70°C, a stirring rate of 100-500r / min, and a stirring time of 0.5-5h.
6. The preparation method according to claim 4 or 5, characterized in that: In the step S2, the silane coupling agent includes at least one of KH560, KH570, KH602, KH550, and KH706; the surface affinity treatment conditions include: temperature of 50-70°C, stirring rate of 100-500 r / min, and stirring time of 1-10 h.
7. The preparation method according to any one of claims 4 to 6, characterized in that: In step S3, the emulsifier includes at least one of OP-10, sodium dodecylbenzene sulfonate, and carboxymethyl cellulose. Preferably, the emulsifier is OP-10, sodium dodecylbenzene sulfonate, and carboxymethyl cellulose in a compound according to (2-4): (4-6): (1-3); the amount of the emulsifier added is 7-13% of the mass of the second product; The emulsification reaction conditions include: temperature of 120-150° C., stirring rate of 500-800 r / min, pressure of 1.5-2 MPa, and emulsification reaction time of 1-2 h.
8. The preparation method according to any one of claims 4 to 7, characterized in that: In the step S4, the amount of tetraethyl orthosilicate added is 240-320% of the mass of the third product; the solvent is water or ethanol; the mixing conditions include: temperature of 120-150°C, stirring rate of 500-800r / min, pH of 3-5, and stirring time of 6-8h.
9. Use of the high temperature resistant phase change microspheres according to any one of claims 1 to 3 or the high temperature resistant phase change microspheres prepared by the preparation method according to any one of claims 4 to 8 in the field of water-based drilling fluids.
10. The use according to claim 9, characterized in that: The mass fraction ratio of the high temperature resistant phase change microspheres in the water-based drilling fluid is 5%-10%.
Citation Information
Cited By
Drilling fluid and preparation method thereof
CN119410347A